Anti-sticking plastic packaging paper and preparation method thereof
By applying an anti-adhesive layer on the upper and lower surfaces of the base paper layer of the plastic-substituted packaging paper, the problems of resin film adhesion and insufficient structural strength are solved, good anti-adhesiveness and structural strength are achieved, and the stability and application value of the packaging paper are improved. .
Patent Information
- Application Number
- CN202411186180.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The existing plastic-based packaging paper has adhesive bonds and insufficient structural strength at high temperatures, resulting in adhesion and damage problems, especially when used in outer packaging.
The anti-adhesion layer is coated on the upper and lower surfaces of the base paper layer, and the components include acrylic resin emulsion, composite fibers, amino silicone oil, vinyl silicone oil and conductive fillers. A low-adhesion film is formed by curing ultraviolet light to enhance anti-adhesion and structural strength.
It achieves good anti-adhesion, structural strength and anti-static functions, improves the tensile and tear resistance of the packaging paper, and enhances the overall stability and application value.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging materials, and in particular to an anti-sticky plastic-substitute packaging paper and a preparation method thereof. Background Art
[0002] Plastic-free paper has the same strength as plastic packaging and can replace plastic packaging to a certain extent. There are two ways to produce plastic-free paper. The first is to add materials or reagents that can increase the strength of paper to the pulp during paper production. The second is to directly apply functional coatings on the paper to form a thin functional film on the surface of the paper, thereby obtaining plastic-free paper that can replace plastic packaging. Because the second method is relatively simple, the production of plastic-free paper also adopts this method. In the above-mentioned functional coatings, the main material is film-forming resin. The film-forming resin includes acrylic Acrylic resin, polyamide resin, etc., enable the functional coating to cover the surface of paper in the form of a film to form a resin film. However, the resin film will soften when the ambient temperature is high. The resin films of the stacked plastic papers will come into contact with each other, and adhesion will occur between the resin films. When the plastic papers that stick to each other are torn apart, the resin film layer may be damaged, causing the resin film layer to separate from the paper layer, making the plastic paper unusable. Therefore, the functional coating coated on the paper needs to have a certain anti-stick (or anti-adhesion) function, that is, to prevent adhesion between the functional film layers of adjacent plastic papers in a stacked state.
[0003] Based on the above situation, in the prior art, the patent with publication number CN117364542A discloses a water- and oil-blocking and anti-rebound food plastic-substitute packaging paper and its preparation method and application. The food plastic-substitute packaging paper adopts a multi-layer composite structure design, including an inner layer, an intermediate layer and a surface layer that are composited in sequence; the inner layer is a base paper layer, the intermediate layer is a starch layer, and the surface layer is a waterproof and oil-proof barrier coating; the waterproof and oil-proof barrier coating is prepared by coating a water-based acrylic resin emulsion and a biodegradable filler; the biodegradable filler can specifically be a biodegradable ester material, and the waterproof and oil-proof barrier coating can block water and oil. The above-mentioned food plastic-substitute packaging paper has good oil-blocking, water-blocking, anti-rebound and other properties.
[0004] However, the above-mentioned plastic substitute packaging paper still has room for improvement in light of actual conditions. The above-mentioned waterproof and oil-proof barrier coating uses biodegradable fillers and is made based on a water-based acrylic resin emulsion, but this coating has not been specifically optimized for anti-adhesion performance, so that the waterproof and oil-proof barrier coating is insufficient to provide sufficient anti-adhesion effect, especially when the packaging paper is stacked or in contact with other objects. At the same time, the above-mentioned plastic substitute packaging paper also has the problem of insufficient structural strength. The waterproof and oil-proof barrier coating and the starch layer are insufficient to provide sufficient structural strength for the above-mentioned plastic substitute packaging paper, so that the above-mentioned plastic substitute packaging paper is only suitable for inner packaging of products and is prone to damage when used as outer packaging. Summary of the invention
[0005] In view of the technical defects existing in the background technology, the present invention proposes an anti-sticky plastic-substitute packaging paper and a preparation method thereof, which solves the above technical problems and meets the actual needs. The specific technical scheme is as follows: An anti-sticky plastic-substitute packaging paper comprises a base paper layer, wherein the upper and lower surfaces of the base paper layer are provided with anti-sticking layers, the anti-sticking layers are made of an anti-sticking coating coated on the surface of the base paper layer, and the thickness of the anti-sticking layers is 30 to 150 μm.
[0006] The fiber coating comprises the following components in parts by weight: 80-90 parts of acrylic resin emulsion, 5-10 parts of composite fiber, 20-50 parts of amino silicone oil, 50-80 parts of vinyl silicone oil, 10-20 parts of conductive filler, 1-5 parts of dispersant and 1-5 parts of photoinitiator.
[0007] The composite fiber is formed by compounding modified glass fiber and chitosan fiber, and the conductive filler is formed by mixing nano conductive particles and multi-walled carbon nanotubes.
[0008] Furthermore, the acrylic resin emulsion is a low molecular weight emulsion type acrylic resin with a molecular weight of 4000-6000, the glass fiber has a length of 200-500 μm and a diameter of 10-20 μm, and the chitosan fiber has a length of 300-500 μm and a diameter of 10-20 μm.
[0009] Furthermore, the nano-conductive particles are selected from any one or more of iron powder, cobalt powder, nickel powder, iron oxide powder, cobalt oxide powder or nickel oxide powder, the weight ratio of the conductive particles to the multi-walled carbon nanotubes in the conductive filler is 1: (2-4), the particle size of the nano-conductive particles is 50-60nm, and the diameter of the multi-walled carbon nanotubes is 30-90nm and the length is 5-10μm.
[0010] Furthermore, the dispersant is selected from any one or more of triethylhexyl phosphate, methylpentanol, and fatty acid polyethylene glycol esters.
[0011] Furthermore, the photoinitiator is selected from any one of benzophenone derivatives or benzophenone.
[0012] A method for making anti-sticky plastic-substitute packaging paper comprises the following steps: S1. Preparing modified glass fiber, preparing an amino coupling agent, methanol and water into a mixed solution, adding glass fiber to the mixed solution and stirring for a period of time, then filtering out the glass fiber, washing, to obtain a modified glass fiber; S2. Preparation of composite fibers, chitosan fibers and modified glass fibers were placed in a beaker containing deionized water, heated, adjusted to pH 8-9.5, and then glutaraldehyde solution was added dropwise for cross-linking reaction, filtered to obtain a fiber intermediate, the fiber intermediate was washed and dried to obtain a composite fiber; S3. The composite fiber, amino silicone oil, vinyl silicone oil, conductive filler, dispersant, photoinitiator are sequentially added to the acrylic emulsion and stirred to obtain a release coating; S4. The anti-sticking coating is applied to the upper and lower surfaces of the base paper layer, irradiated with ultraviolet light, and then dried and cut to obtain an anti-sticky plastic-substitute packaging paper.
[0013] Furthermore, in step S1, the amino coupling agent is selected from any one of 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane or 3-aminopropyltriethoxysilane.
[0014] Furthermore, in step S1, the glass fiber is added to a mixed solution of 50-60 times the volume, and stirred and immersed for 30-40 minutes, the glass fiber is filtered out, washed, and dried to obtain modified glass fiber, and the weight percentage of each component in the mixed solution is: amino coupling agent 1%-5%, methanol 80%-95%, and deionized water 19%-5%.
[0015] Furthermore, in step S2, 2.0-5.0 g of chitosan fiber and modified glass fiber are weighed respectively, put into a beaker containing 100 ml of deionized water, stirred and heated to 50°C, 0.1 mol / L sodium hydroxide solution is used to adjust the pH to 8.5, and then 5-10 ml of a 40-50% by mass glutaraldehyde aqueous solution is slowly added under stirring conditions, reacted for 1-2 hours, filtered, and a fiber intermediate is obtained. The fiber intermediate is washed and dried to obtain a composite fiber.
[0016] Furthermore, in step S4, the method of curing by UV lamp is as follows: the UV lamp is 10-15 cm away from the anti-sticking layer, the power of the UV lamp is 5000-15000 mW / cm², and the irradiation time of the anti-sticking coating under the UV lamp is 3-10 s.
[0017] The beneficial effects of the present invention are: The plastic substitute packaging paper of the present invention has good anti-adhesion, structural strength and anti-static function. Anti-adhesion layers are arranged on the upper and lower surfaces of the base paper layer, and components such as acrylic resin emulsion, amino silicone oil, vinyl silicone oil and the like in the anti-adhesion coating work together to form a low-viscosity film on the surface of the packaging paper. Amino silicone oil and vinyl silicone oil can increase the lubricity and low surface tension of the surface of the plastic substitute packaging paper, and can reduce the friction coefficient of the surface of the packaging paper to prevent adhesion. The composite fiber is formed by composite of modified glass fiber and chitosan fiber, which effectively improves the physical properties of the anti-stretching, anti-tearing and the like of the anti-adhesion layer, and at the same time enhances the structural strength of the entire packaging paper. The plastic substitute packaging paper can better resist external forces during transportation, storage and use, and maintain its integrity and stability. Conductive fillers mixed with nano-conductive particles and multi-walled carbon nanotubes are added to the adhesive coating, and the conductive fillers are evenly distributed in the coating to form a conductive network, so that the anti-adhesion layer has good anti-static properties. DETAILED DESCRIPTION
[0018] The implementation mode of the present invention is described below in conjunction with relevant embodiments. The implementation mode of the present invention is not limited to the following embodiments, and the present invention relates to relevant necessary components in the technical field, which should be regarded as the known technology in the technical field and can be known and mastered by the technical personnel in the technical field.
[0019] An anti-sticky plastic-substitute packaging paper comprises a base paper layer, wherein the upper and lower surfaces of the base paper layer are provided with anti-sticking layers, the anti-sticking layers are made of an anti-sticking coating coated on the surface of the base paper layer, and the thickness of the anti-sticking layers is 30 to 150 μm.
[0020] The fiber coating comprises the following components in parts by weight: 80-90 parts of acrylic resin emulsion, 5-10 parts of composite fiber, 20-50 parts of amino silicone oil, 50-80 parts of vinyl silicone oil, 10-20 parts of conductive filler, 1-5 parts of dispersant and 1-5 parts of photoinitiator.
[0021] The composite fiber is formed by compounding modified glass fiber and chitosan fiber, and the conductive filler is formed by mixing nano conductive particles and multi-walled carbon nanotubes.
[0022] The anti-sticking layer of the present invention uses acrylic resin emulsion as a base material, which provides the main film-forming property and adhesion for the anti-sticking layer. Under the action of a photoinitiator, the acrylic resin emulsion can undergo a cross-linking reaction to form a stable network structure, thereby enhancing the mechanical strength and weather resistance of the anti-sticking layer. At the same time, the acrylic resin emulsion is combined with components such as vinyl silicone oil and amino silicone oil to form a more compact and stable anti-sticking layer through a cross-linking reaction, thereby improving the overall performance. The vinyl silicone oil has excellent lubricity and low surface tension, and can effectively reduce the friction coefficient of the packaging paper surface and reduce adhesion. The amino silicone oil not only has lubricity, but can also form a hydrogen bond connection with the grid structure formed by the acrylic resin emulsion, thereby further enhancing the flexibility and stability of the anti-sticking layer.
[0023] The composite fiber is made of chitosan fiber and modified glass fiber cross-linked by glutaraldehyde, which significantly enhances the overall structural strength of the anti-adhesive layer and the plastic substitute paper. The chitosan fiber has good biocompatibility and degradability, which increases the environmental performance of the plastic substitute paper. The composite fiber is used as a reinforcing material for the anti-adhesive layer. The composite fiber improves the mechanical properties of the anti-tear and anti-puncture of the anti-adhesive layer. The grid structure formed by the cross-linking of the composite fiber, acrylic resin emulsion and vinyl silicone oil works together to form a more stable and durable anti-adhesive system and a high-strength structural system. The nano-conductive particles and multi-walled carbon nanotubes of the conductive filler form a conductive network in the anti-adhesive layer to increase the conductive performance. The conductive network can quickly transfer the static electricity on the surface to the anti-adhesive layer and dissipate it, thereby giving the anti-adhesive layer good antistatic performance. Thereby improving the application value of plastic substitute packaging paper in the fields of electronic products, medical packaging, etc.
[0024] As one of the preferred embodiments of the present invention, the acrylic resin emulsion is a low molecular weight emulsion type acrylic resin with a molecular weight of 4000-6000, the glass fiber has a length of 200-500 μm and a diameter of 10-20 μm, and the chitosan fiber has a length of 300-500 μm and a diameter of 10-20 μm.
[0025] The molecular weight of the acrylic resin emulsion of the present invention is preferably 4000. The acrylic resin has the advantages of fast curing speed, excellent film-forming performance, wide applicability, etc. The acrylic resin can quickly undergo polymerization reaction under ultraviolet light irradiation, thereby achieving rapid curing. The excellent film-forming performance can enable the anti-sticking layer to exhibit good wear resistance and chemical corrosion resistance. At the same time, the acrylic resin has good adhesion and can be closely combined with other types of components when mixed with other types of components. Compared with high molecular weight acrylic resin, low molecular weight acrylic resin has lower viscosity, better fluidity and shorter curing time. Lower viscosity is conducive to the mixing of components such as conductive fillers and composite fibers in the acrylic resin emulsion.
[0026] The diameters of the glass fibers and chitosan fibers of the present invention are both 300 μm and 10 μm, respectively. When the lengths of the glass fibers and chitosan fibers are both controlled at 300 μm and the diameters are both controlled at 10 μm, the combination of the glass fibers and the chitosan fibers is more uniform in structure, which helps to better interweave and combine the glass fibers and the chitosan fibers during the subsequent preparation of the composite fibers, thereby improving the overall strength and stability of the composite fibers.
[0027] As one of the preferred embodiments of the present invention, the nano conductive particles are selected from any one or more of iron powder, cobalt powder, nickel powder, iron oxide powder, cobalt oxide powder or nickel oxide powder, the weight ratio of the conductive particles to the multi-walled carbon nanotubes in the conductive filler is 1: (2-4), the particle size of the conductive particles is 50-60nm, and the diameter of the multi-walled carbon nanotubes is 30-90nm and the length is 5-10μm.
[0028] The nano-conductive particles of the present invention use cobalt powder with a particle size of 50nm, and the weight ratio of cobalt powder to multi-walled carbon nanotubes in the conductive filler is 1:3. The cobalt powder effectively improves the conductive efficiency of the anti-sticking layer with its good conductive performance, so that static electricity can be transmitted quickly and efficiently. The weight ratio of cobalt powder to multi-walled carbon nanotubes is 1:3, which ensures the density and continuity of the conductive network. The multi-walled carbon nanotubes serve as conductive bridges, further enhancing the connection between the conductive particles and improving the overall conductive performance. The larger diameter of the multi-walled carbon nanotubes helps to form a more stable conductive network structure and improves the mechanical strength and durability of the anti-sticking layer.
[0029] As one of the preferred embodiments of the present invention, the dispersant is selected from any one or more of triethylhexyl phosphoric acid, methylpentanol, and fatty acid polyethylene glycol esters.
[0030] The dispersant of the present invention is fatty acid polyethylene glycol ester, which is a highly efficient dispersant and can reduce the surface tension between the components in the anti-stick coating, so that raw materials such as acrylic resin emulsion, composite fiber, amino silicone oil, vinyl silicone oil, conductive filler, etc. are more easily dispersed evenly during the mixing process, avoiding the occurrence of agglomeration and precipitation, thereby ensuring the uniformity and consistency of the anti-stick coating. At the same time, the addition of fatty acid polyethylene glycol ester also helps to improve the bonding force between the anti-sticking layer and the base paper layer, so that the anti-sticking layer is more firmly attached to the base paper layer, thereby improving the overall strength and durability of the plastic-substitute packaging paper.
[0031] As one of the preferred embodiments of the present invention, the photoinitiator is selected from any one of benzophenone derivatives or benzophenone; the photoinitiator is preferably 4,4'-dichlorobenzophenone, which is a derivative of benzophenone. 4,4'-dichlorobenzophenone has the characteristics of good stability, high photosensitivity, and fast curing speed in photocuring applications. At the same time, there is no need to add tertiary amine substances as co-initiators during the resin curing process. The combined use of acrylic resin and 4,4'-dichlorobenzophenone can effectively improve the coating efficiency of the anti-sticking coating.
[0032] A method for making anti-sticky plastic-substitute packaging paper comprises the following steps: S1. Prepare modified glass fiber, prepare a mixed solution of amino coupling agent, methanol and water, add glass fiber into the mixed solution and stir for a period of time, then filter out the glass fiber, wash it, and obtain modified glass fiber.
[0033] S2. Prepare composite fiber, put chitosan fiber and modified glass fiber into a beaker containing deionized water, heat, adjust pH=8-9.5, then drop glutaraldehyde solution to carry out cross-linking reaction, filter to obtain fiber intermediate, wash and dry the fiber intermediate to obtain composite fiber.
[0034] S3. The composite fiber, amino silicone oil, vinyl silicone oil, conductive filler, dispersant, and photoinitiator are sequentially added to the acrylic emulsion and stirred evenly to obtain a release coating.
[0035] S4. The anti-sticking coating is applied to the upper and lower surfaces of the base paper layer, irradiated with ultraviolet light, and then dried and cut to obtain an anti-sticky plastic-substitute packaging paper.
[0036] In the manufacturing method of the plastic substitute packaging paper of the present invention, various functional ingredients such as composite fibers, amino silicone oil, vinyl silicone oil, conductive fillers, etc. are uniformly dispersed in acrylic emulsion to form an anti-sticking layer coating with high anti-sticking, high conductivity and high strength characteristics. The glass fiber is surface treated with an amino coupling agent to effectively improve the interface performance of the glass fiber. In the preparation process of the composite fiber, chitosan fiber, modified glass fiber and glutaraldehyde undergo a cross-linking reaction to form a composite fiber with good mechanical properties. The composite fiber is in the anti-sticking layer to enhance the structural strength of the anti-sticking layer, so that the plastic substitute packaging paper can better resist the influence of the external environment during use. In the coating and curing stages, ultraviolet light irradiation curing technology is adopted, which not only improves the production efficiency but also ensures the rapid curing and molding of the anti-sticking layer coating. UV light irradiation causes the acrylic resin emulsion and vinyl silicone oil to rapidly undergo a cross-linking reaction under the action of the photoinitiator, forming a stable three-dimensional network structure. At the same time, hydrogen bonds are formed between the amino silicone oil and the grid structure, further enhancing the structural strength of the coating. In addition, multi-walled carbon nanotubes construct an efficient conductive network in the anti-sticking layer, allowing surface static electricity to be quickly transmitted and dissipated, thereby giving the plastic-free packaging paper excellent anti-static properties.
[0037] As one of the preferred embodiments of the present invention, in step S1, the glass fiber is added to a mixed solution of 50-60 times the volume, and stirred and immersed for 30-40 minutes, the glass fiber is filtered out, washed, and dried to obtain modified glass fiber, and the weight percentage of each component in the mixed solution is: amino coupling agent 1%-5%, methanol 80%-95%, and deionized water 19%-5%; in step S1, the amino coupling agent is selected from any one of 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane or 3-aminopropyltriethoxysilane.
[0038] The amino coupling agent of the present invention is 3-aminopropyltrimethoxysilane, and the weight percentages of the components in the aqueous solution of the amino coupling agent in methanol are: 1% of the amino coupling agent, 90% of methanol, and 9% of deionized water; The present invention selects 3-aminopropyltrimethoxysilane as an amino coupling agent, and mixes it with methanol and deionized water in a certain ratio to form a treatment solution for modified glass fiber. 3-aminopropyltrimethoxysilane is used to introduce amino functional groups on the surface of glass fiber, thereby improving the compatibility and bonding force between glass fiber and other materials. The trimethoxysilane part of 3-aminopropyltrimethoxysilane can undergo condensation reaction with hydroxyl groups on the surface of glass fiber, thereby forming a stable chemical bond on the surface of glass fiber, and the 3-aminopropyl part provides an amino functional group for subsequent reaction with shell polymer. The cross-linking reaction of organic materials such as sugar fiber creates conditions. In the process of preparing modified glass fiber, the glass fiber is added into a mixed solution containing 3-aminopropyltrimethoxysilane, methanol and deionized water, and after stirring and impregnation treatment, the silane coupling agent molecules gradually penetrate into the surface and interior of the glass fiber, and combine with the hydroxyl groups on the surface of the glass fiber through hydrolysis and condensation reactions, thereby introducing a large number of amino functional groups on the surface of the glass fiber. After filtering, washing and drying, the surface of the modified glass fiber is covered with a layer of silane coupling agent containing amino functional groups.
[0039] As one of the preferred embodiments of the present invention, in step S2, 2.0-5.0 g of chitosan fiber and modified glass fiber are weighed respectively, put into a beaker containing 100 ml of deionized water, stirred and heated to 50°C, 0.1 mol / L sodium hydroxide solution is used to adjust the pH to 8.5, and then 5-10 ml of a 40-50% mass fraction glutaraldehyde aqueous solution is slowly added under stirring conditions, reacted for 1-2 hours, filtered, and a fiber intermediate is obtained. The fiber intermediate is washed and dried to obtain a composite fiber.
[0040] In step S2, 2.0 g of chitosan fiber and modified glass fiber are weighed respectively, put into a beaker containing 100 ml of deionized water, stirred and heated to 50°C, 0.1 mol / L sodium hydroxide solution is used to adjust the pH to 8.5, and then 5 ml of 50% by mass glutaraldehyde aqueous solution is slowly added under stirring conditions, reacted for 1 hour, filtered to obtain a fiber intermediate, and the fiber intermediate is washed and dried to obtain a composite fiber.
[0041] In step S2, glutaraldehyde is used as a cross-linking agent to promote the strong bonding between the modified glass fiber and the chitosan fiber under alkaline conditions (pH=8.5). The surfaces of the modified glass fiber and the chitosan fiber contain amino functional groups, which are easy to react with glutaraldehyde molecules in an alkaline environment. The aldehyde groups in the glutaraldehyde molecules can undergo condensation reaction with the amino groups to form a stable Schiff base structure, thereby tightly cross-linking the modified glass fiber and the chitosan fiber together. In step S1, the modified glass fiber is treated with an amino coupling agent to introduce amino functional groups on its surface, thereby enhancing the reactivity of the fiber. At the same time, the chitosan fiber itself also contains abundant amino and hydroxyl groups. When the modified glass fiber, chitosan, glutaraldehyde, and sodium hydroxide solution are placed in a beaker and heated to 50°C, the aldehyde groups in the glutaraldehyde molecules begin to undergo condensation reactions with the amino groups on the surfaces of the two fibers to form stable covalent bonds.
[0042] As one of the preferred embodiments of the present invention, in step S4, the method of curing by UV lamp is as follows: the UV lamp is 10-15 cm away from the anti-sticking layer, the power of the UV lamp is 5000-15000 mW / cm², and the irradiation time of the anti-sticking coating under the UV lamp is 3-10 s.
[0043] In step S4, the UV lamp is placed 10 cm away from the anti-adhesive layer, ensuring that the UV light can fully irradiate the surface of the anti-adhesive layer, while avoiding overheating or excessive light intensity that damages the material due to being too close. At the same time, the power range of the UV lamp is set to 10000mW / cm². The high power setting ensures that the UV light can provide sufficient energy in a short time to promote the rapid cross-linking reaction of the acrylic resin emulsion and the vinyl silicone oil under the action of the photoinitiator to form a stable three-dimensional network structure. In addition, the irradiation time of the anti-adhesive coating under the UV lamp is controlled within 10s. The short exposure time not only improves the production efficiency, but also effectively prevents the aging or degradation of the coating caused by long-term exposure.
[0044] Example 1
[0045] S1. Prepare modified glass fiber by mixing 3-aminopropyltrimethoxysilane, methanol and deionized water in the following proportions: 1% amino coupling agent, 90% methanol, 9% deionized water to form a uniform solution. Then, add glass fiber to the mixed solution to ensure that the glass fiber is fully impregnated. The added amount is 60 times the volume of the mixed solution, and stirred and impregnated for 30 minutes.
[0046] S2. Prepare composite fibers. Place 2.0 g of chitosan fiber and modified glass fiber into a beaker filled with deionized water, heat to 50°C and adjust the pH of the solution to 8.5 (using 0.1 mol / L sodium hydroxide solution). Slowly add 5 ml of 50% glutaraldehyde aqueous solution into the beaker. The reaction time is 1 hour. Then filter, wash and dry to obtain composite fibers.
[0047] S3. Prepare a release coating by adding 5 parts of composite fiber, 20 parts of amino silicone oil, 50 parts of vinyl silicone oil, 10 parts of conductive filler, 1 part of dispersant, and 1 part of photoinitiator to 90 parts of acrylic resin emulsion and stirring well to form a release coating.
[0048] S4. Coating and curing: The prepared anti-sticking coating is evenly coated on the upper and lower surfaces of the base paper layer with a coating thickness of 100 microns. Subsequently, a UV lamp is used for irradiation and curing. The UV lamp is 10 cm away from the anti-sticking layer, the power is set to 10,000 mW / cm², and the irradiation time is controlled within 10 seconds. Finally, after drying and cutting, an anti-sticky plastic-substitute packaging paper is obtained.
[0049] The anti-sticking plastic packaging paper was tested for anti-sticking, surface resistance, and anti-puncture performance. The anti-sticking test was conducted in a high temperature and high humidity test chamber (62°C, 60% humidity, two pieces of plastic packaging paper were put together, a load was applied so that the paper was subjected to a pressure of 500Pa, and it was left to stand for 24 hours) to observe the anti-sticking phenomenon.
[0050] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the glass fibers and chitosan fibers in the composite fibers are not cross-linked.
[0051] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that no multi-walled carbon nanotubes are added in Comparative Example 2.
[0052] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that no conductive particles are added in Comparative Example 3.
[0053] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that amino silicone oil and vinyl silicone oil are not added in Comparative Example 4.
[0054]
[0055] Comparison between Example 1 and Comparative Example 1 shows that whether or not to crosslink the glass fiber and chitosan fiber has no significant effect on the anti-sticking phenomenon, and both show no anti-sticking phenomenon. This may be because crosslinking mainly affects the bonding strength between the fibers, but has little effect on the anti-sticking performance of the final product. Comparative Example 4 (without adding amino silicone oil and vinyl silicone oil) has obvious anti-sticking phenomenon, which illustrates the key role of amino silicone oil and vinyl silicone oil in the anti-sticking layer coating, effectively reducing the adhesion of the material and preventing the occurrence of anti-sticking phenomenon.
[0056] The surface resistance of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 is 10 5 Ω to 10 8 Ω range, indicating that Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 have certain electrical conductivity or electrostatic dissipation capabilities, among which the surface resistance of Comparative Example 2 (without adding multi-walled carbon nanotubes) is slightly lower than that of other groups, indicating that although multi-walled carbon nanotubes have a certain effect on electrical conductivity.
[0057] The puncture resistance of Example 1 is the highest (20.1N), while the puncture resistance of Comparative Example 2 (without adding multi-walled carbon nanotubes) is significantly reduced (17.5N), indicating that multi-walled carbon nanotubes have a significant effect on improving the puncture resistance of the material, because carbon nanotubes have high strength and excellent mechanical properties and can enhance the overall strength of the composite material. Although the puncture resistance of Comparative Example 1 (without cross-linking), Comparative Example 3 (without adding conductive particles) and Comparative Example 4 (without adding amino silicone oil and vinyl silicone oil) is slightly lower than that of Example 1, it indicates that these changes have relatively little effect on the puncture resistance.
[0058] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An anti-sticky plastic packaging paper, characterized in that: It comprises a base paper layer, wherein the upper and lower surfaces of the base paper layer are provided with anti-sticking layers, wherein the anti-sticking layers are made of an anti-sticking coating coated on the surface of the base paper layer, and the thickness of the anti-sticking layers is 30 to 150 μm; The fiber coating comprises the following components in parts by weight: 80-90 parts of acrylic resin emulsion, 5-10 parts of composite fiber, 20-50 parts of amino silicone oil, 50-80 parts of vinyl silicone oil, 10-20 parts of conductive filler, 1-5 parts of dispersant, and 1-5 parts of photoinitiator; The composite fiber is formed by compounding modified glass fiber and chitosan fiber, and the conductive filler is formed by mixing nano conductive particles and multi-walled carbon nanotubes.
2. The anti-stick plastic packaging paper according to claim 1, characterized in that: The acrylic resin emulsion is a low molecular weight emulsion type acrylic resin with a molecular weight of 4000-6000. The glass fiber has a length of 200-500 μm and a diameter of 10-20 μm. The chitosan fiber has a length of 300-500 μm and a diameter of 10-20 μm.
3. The anti-sticky plastic packaging paper according to claim 1, characterized in that: The nano conductive particles are selected from any one or more of iron powder, cobalt powder, nickel powder, iron oxide powder, cobalt oxide powder or nickel oxide powder. The weight ratio of the conductive particles to the multi-walled carbon nanotubes in the conductive filler is 1: (2-4). The particle size of the conductive particles is 50-60nm, and the diameter of the multi-walled carbon nanotubes is 30-90nm and the length is 5-10μm.
4. The anti-sticky plastic packaging paper according to claim 1, characterized in that: The dispersant is selected from any one or more of triethylhexyl phosphoric acid, methylpentanol, and fatty acid polyethylene glycol ester.
5. The anti-sticky plastic packaging paper according to claim 1, characterized in that: The photoinitiator is selected from any one of benzophenone derivatives or benzophenone.
6. A method for making an anti-sticky plastic-replacing packaging paper as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Preparing modified glass fiber, preparing an amino coupling agent, methanol and water into a mixed solution, adding glass fiber to the mixed solution and stirring for a period of time, then filtering out the glass fiber, washing, to obtain a modified glass fiber; S2. Preparation of composite fibers, chitosan fibers and modified glass fibers were placed in a beaker containing deionized water, heated, adjusted to pH 8-9.5, and then glutaraldehyde solution was added dropwise for cross-linking reaction, filtered to obtain a fiber intermediate, the fiber intermediate was washed and dried to obtain a composite fiber; S3. The composite fiber, amino silicone oil, vinyl silicone oil, conductive filler, dispersant, photoinitiator are sequentially added to the acrylic emulsion and stirred to obtain a release coating; S4. The anti-sticking coating is applied to the upper and lower surfaces of the base paper layer, irradiated with ultraviolet light, and then dried and cut to obtain an anti-sticky plastic-substitute packaging paper.
7. The method for making the anti-sticky plastic-substitute packaging paper according to claim 6, characterized in that: In step S1, the amino coupling agent is selected from any one of 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane or 3-aminopropyltriethoxysilane.
8. The method for making the anti-sticky plastic-substitute packaging paper according to claim 6, characterized in that: In step S1, the glass fiber is added to a mixed solution of 50-60 times the volume, and stirred and immersed for 30-40 minutes, the glass fiber is filtered out, washed, and dried to obtain modified glass fiber, and the weight percentage of each component in the mixed solution is: amino coupling agent 1%-5%, methanol 80%-95%, and deionized water 19%-5%.
9. The method for making the anti-sticky plastic-substitute packaging paper according to claim 6, characterized in that: In step S2, 2.0-5.0 g of chitosan fiber and modified glass fiber are weighed respectively, put into a beaker containing 100 ml of deionized water, stirred and heated to 50°C, 0.1 mol / L sodium hydroxide solution is used to adjust the pH to 8.5, and then 5-10 ml of a 40-50% mass fraction glutaraldehyde aqueous solution is slowly added under stirring conditions, reacted for 1-2 hours, filtered, and a fiber intermediate is obtained. The fiber intermediate is washed and dried to obtain a composite fiber.
10. The method for making the anti-sticky plastic-substitute packaging paper according to claim 6, characterized in that: In step S4, the method of curing by UV lamp is as follows: the UV lamp is 10-15 cm away from the anti-sticking layer, the power of the UV lamp is 5000-15000 mW / cm², and the irradiation time of the anti-sticking coating under the UV lamp is 3-10 s.