Paper core with high outer layer flexibility and high inner layer hardness and preparation method thereof
By using multi-layer structure and specific antibacterial flame retardant glue in the paper core, the problems of easy cracking and insufficient glue performance during winding are solved, and high radial pressure tolerance, excellent antibacterial and flame retardant performance and low water content are achieved. Green and environmentally friendly paper core.
Patent Information
- Application Number
- CN202411176481.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
Existing paper cores are prone to rupture when wrapping fragile rolls such as photo paper or aluminum foil, and the adhesive strength, flame retardancy and antibacterial properties of the glue are insufficient, which affects product performance.
The paper core design adopts a multi-layer structure, including hard kraft paper layer, antibacterial flame retardant glue layer, foam paper layer and soft kraft paper layer. The antibacterial flame retardant glue is composed of modified corn starch, phenolic resin, flame retardant, antibacterial agent and other components. Composition, improves adhesive performance and flame retardant effect through modification treatment.
The paper core has high radial pressure tolerance, excellent antibacterial and flame retardant properties, low moisture content and green environmental protection characteristics, ensuring the stability and safety of the product.
Smart Images

Figure BDA0005010859810000091 
Figure BDA0005010859810000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of paper tube processing, and in particular to a paper core with high flexibility in the outer layer and high hardness in the inner layer and a preparation method thereof. Background Art
[0002] With the rapid economic development, industrial development has also entered an unprecedented height, and the demand for auxiliary materials required for industrial development has gradually increased. The use of paper tubes has become more and more extensive, and the amount of paper tubes has also increased. Paper tubes refer to tubular objects made of paper, which are widely used in the carrying packaging of various films.
[0003] In the printing and packaging industries, paper cores are often used as support for the storage and transportation of rolls of materials such as photo paper or aluminum foil. Existing paper cores are mostly composed of a single layer of kraft paper, which has very high strength and hardness. However, when winding fragile rolls such as photo paper or aluminum foil, a paper core with too high a hardness may cause the roll to break.
[0004] Glue is used when preparing multi-layer paper cores. Current glue has poor bonding strength, flame retardancy, and antibacterial properties, and the glue easily penetrates into the foam paper, affecting the performance of the product. Summary of the invention
[0005] The purpose of this application is to provide a paper core with high outer flexibility and high inner hardness and a preparation method thereof in view of the shortcomings of the current technology. The preparation method of the paper core with high outer flexibility and high inner hardness of the application has the advantages of simple preparation and low cost, and the paper core with high outer flexibility and high inner hardness has high radial pressure, is green, environmentally friendly and safe, and has a low moisture content (6-7%). The antibacterial flame retardant glue prepared by the application has excellent antibacterial properties, flame retardancy and bonding strength, and is also highly safe and environmentally friendly.
[0006] In the first aspect, the present application provides a paper core with high flexibility in the outer layer and high hardness in the inner layer, adopting the following technical scheme: a paper core with high flexibility in the outer layer and high hardness in the inner layer, comprising, from the inside to the outside, a hard kraft paper layer, an antibacterial flame retardant glue layer, a foam paper layer and a soft kraft paper layer, wherein the antibacterial flame retardant glue layer is prepared by coating the antibacterial flame retardant glue on the surface of the hard kraft paper layer and bonding the foam paper layer, wherein the antibacterial flame retardant glue, measured by mass, comprises the following preparation raw materials: 60-70 parts of modified corn starch, 3-5 parts of phenolic resin, 5-7 parts of flame retardant, 3-4 parts of antibacterial agent, 0.3-0.5 parts of urethane acrylate, 0.2-0.3 parts of hypotonic agent, 0.3-0.4 parts of preservative, and 300-330 parts of water.
[0007] By adopting the above technical scheme, the hard kraft paper layer: as the inner layer of the paper core, it provides hardness and support to ensure the structural stability of the paper core. The antibacterial flame retardant glue layer: the antibacterial flame retardant glue is coated on the surface of the hard kraft paper layer to bond the foam paper layer. The antibacterial flame retardant glue has excellent antibacterial properties, flame retardancy and bonding strength, which can effectively prevent bacterial growth and flame spread, and at the same time firmly bond the foam paper layer to the hard kraft paper layer. The foam paper layer: located outside the antibacterial flame retardant glue layer, provides buffering and protection, and increases the flexibility and impact resistance of the paper core. The soft kraft paper layer: as the outer layer of the paper core, it has high flexibility, can adapt to various bending and deformation, and protect the internal structure from damage. Modified corn starch: modified by 3-chloro-2-hydroxypropyl-trimethylammonium chloride, the side chain is increased, the compatibility with the resin is improved, and the antibacterial flame retardant glue has better bonding properties. Phenolic resin: as the main component of the adhesive, it provides bonding force and firmly bonds the layers of materials together. Flame retardant: By activating bentonite and grafting soy protein, the dispersibility of bentonite in the matrix material is improved, and the flame retardant performance is exerted during combustion. 2-Carboxyethylphenyl hypophosphite is used as a gas source to promote the flame retardant to form a foam layer, release a large amount of non-flammable gas, and dilute the oxygen in the environment; sodium alginate forms a viscous aqueous solution with the water produced by combustion, isolates the combustion products and inhibits further combustion. The three synergistically improve the flame retardant effect. Antibacterial agent: It gives the antibacterial flame retardant glue excellent antibacterial properties and effectively prevents bacterial growth. Amino ester acrylate: As a cross-linking agent, it improves the water resistance and weather resistance of the antibacterial flame retardant glue. Low permeability agent: It is a corn starch graft copolymer with extremely low surface energy, which reduces the permeability of the antibacterial flame retardant glue inside the paper, accelerates the drying speed, and improves the bonding strength. Preservative: It extends the service life of the paper core and prevents degradation and damage caused by the growth of bacteria and mold. Water: As a solvent, it adjusts the viscosity and fluidity of the antibacterial flame retardant glue to facilitate coating and bonding. In summary, the paper core of the present application achieves excellent properties such as high radial pressure, green environmental protection and safety, and low moisture content through the synergistic effect of multi-layer structure and specific materials.
[0008] Preferably, the inner diameter of the paper core is 77-80 mm, the thickness is 5-6 mm, the thickness of the hard kraft paper layer is 0.5-1 mm, the thickness of the soft kraft paper layer is 0.5-1 mm, and the thickness of the foam paper layer is 4-5 mm.
[0009] Preferably, the method for preparing the modified corn starch comprises the following steps: S31, according to the mass fraction, dissolve 10 parts of corn starch in 30 parts of deionized water, stir evenly, heat to 40°C, stir while heating, stir for 40 minutes, continue to heat to 48°C, keep for 25 minutes, cool to room temperature, and obtain a mixed solution; S32. Add 0.5 parts of 3-chloro-2-hydroxypropyl-trimethylammonium chloride to the mixed solution according to the mass fraction, stir evenly, microwave the mixed substance for 3 minutes, centrifuge and vacuum dry at 80° C. for 24 hours to obtain modified corn starch.
[0010] By adopting the above technical scheme, S31, pretreatment of corn starch: This step includes mixing corn starch with deionized water, and fully expanding and dispersing the starch granules by heating and stirring. Heating to 40°C and maintaining for a certain period of time helps the swelling and gelatinization of starch granules, and then heating to 48°C and maintaining, which may be to further promote the structural changes of starch granules and make them easier for subsequent chemical modification. The mixed solution obtained after cooling to room temperature provides a uniform reaction medium for the subsequent chemical modification. S32, chemical modification: In this step, 3-chloro-2-hydroxypropyl-trimethylammonium chloride is added to the pretreated starch mixture as a modifier. The amount of modifier added is relatively small, which may mean that only a few hydroxyl groups on each starch molecule are replaced, thereby maintaining the basic structure of starch. Microwave treatment is used to provide rapid and uniform heating to promote the reaction between the modifier and the starch molecules. The short microwave treatment time indicates that the reaction efficiency is high. The subsequent centrifugation and vacuum drying process is used to remove unreacted chemicals and moisture to obtain the final modified corn starch product. Modified corn starch increases compatibility with resins, especially phenolic resins, by grafting 3-chloro-2-hydroxypropyl-trimethylammonium chloride. This helps to improve the overall performance of antibacterial flame retardant glue, ensure good interaction between the components, and thus improve the bonding strength and durability of the paper core. As one of the main ingredients in antibacterial flame retardant glue, modified corn starch's excellent bonding properties help to firmly bond the foam paper layer to the hard kraft paper layer, while providing the required flexibility and hardness to the paper core. Modified corn starch is a renewable resource, and its use is in line with the principle of green environmental protection. In addition, modified corn starch itself is biodegradable and will not cause long-term pollution to the environment. The combination of modified corn starch and hypopermeability agent can effectively prevent the antibacterial flame retardant glue from excessively penetrating into the paper, which not only speeds up the drying speed of the antibacterial flame retardant glue, but also improves the bonding strength and ensures the overall performance of the paper core. In summary, modified corn starch plays multiple roles in the preparation of paper core, including improving compatibility, enhancing bonding properties, ensuring environmental protection and safety, and synergizing with hypotonic agents to improve production efficiency and product quality.
[0011] Preferably, the method for preparing the flame retardant comprises the following steps: S41, placing bentonite in a ball mill, ball milling at 400 rpm for 2 h and passing through a 100 mesh sieve; then placing in a muffle furnace, preheating at 260° C. for 35 min, heating to 1020° C., calcining for 2.5 h, and cooling to room temperature to obtain activated bentonite; S42, according to the mass fractions, 100 parts of activated bentonite and 200 parts of sodium hydroxide aqueous solution with a mass concentration of 12% were mixed and allowed to stand for 4 hours; heated to 85° C. and stirred for reaction for 6 hours; cooled, filtered, and the filter residue was collected; the filter residue was washed with water until the pH value of the filtrate was 7, and dried at 105° C. for 12 hours to obtain microporous bentonite; S43, dissolving 100 parts of microporous bentonite and 20 parts of soy protein in 1200 parts of water according to their weight, stirring and reacting at 3000 rpm for 15 hours; filtering, collecting the filter residue, and drying the filter residue at 105° C. for 10 hours to obtain soy protein modified microporous bentonite; S44. Disperse 100 parts of soy protein modified microporous bentonite, 15 parts of sodium alginate and 200 parts of 2-carboxyethylphenyl hypophosphorous acid in water according to their mass proportions, and add the dispersed mixture into a ball mill at a rotor speed of 3000 rpm. Mill the mixture at room temperature for 4 h, centrifuge the mixture at 35000 rpm for 20 min, collect the precipitate, and then dry the precipitate at 85°C for 7 h to obtain a flame retardant.
[0012] By adopting the above technical scheme, the preparation method of the flame retardant involves multiple steps, including activation of bentonite, preparation of microporous bentonite, modification of soy protein and synthesis of the final composite flame retardant. These steps are aimed at improving the dispersibility and flame retardant properties of bentonite, and further enhancing its flame retardant effect by adding sodium alginate and 2-carboxyethylphenyl hypophosphite. Activation of bentonite (S41): The ball milling and calcination process increases the specific surface area of bentonite and creates more microporous structures, which helps to improve its performance as a flame retardant. High-temperature calcination removes impurities in bentonite and activates its surface, making it more suitable for reacting with other compounds. Preparation of microporous bentonite (S42): The reaction with sodium hydroxide further increases the microporosity of bentonite, which can adsorb and fix flammable gases and reduce the flammability of the material. This step also helps to improve the grafting efficiency of bentonite and soy protein. Soy protein modified microporous bentonite (S43): The introduction of soy protein increases the thermal stability and carbon-forming ability of bentonite, which forms a protective layer during combustion, isolates oxygen and prevents the spread of fire. The amino groups of protein may react with the surface functional groups of bentonite, enhancing the overall flame retardant properties of the material. Synthesis of composite flame retardant (S44): After adding sodium alginate and 2-carboxyethylphenyl hypophosphite, a uniform mixture is obtained through ball milling and centrifugation. Sodium alginate forms a viscous aqueous solution during combustion, isolating the combustion products and inhibiting further combustion. 2-carboxyethylphenyl hypophosphite, as a gas source, promotes the flame retardant to form a foam layer, release non-combustible gas and dilute oxygen. The modified bentonite is evenly dispersed in the paper core, and its microporous structure and the carbon-forming ability of soy protein significantly improve the flame retardant properties of the paper core. The addition of sodium alginate and 2-carboxyethylphenyl hypophosphite, together with bentonite and soy protein, form an efficient flame retardant system, which not only improves the flame retardancy, but also increases the smoke density and carbon layer strength of the material. All raw materials used are environmentally friendly materials, ensuring the safety and environmental friendliness of the paper core during production and use. In summary, this method of preparing flame retardants uses multi-step chemical and physical treatments to give bentonite excellent flame retardant properties, and synergizes with other components to provide an efficient and environmentally friendly flame retardant solution for paper cores.
[0013] Preferably, the antibacterial agent is silver-loaded silicon powder.
[0014] Preferably, the preparation method of the silver-loaded silicon micropowder is as follows: according to the mass fraction, 50 parts of silicon micropowder are soaked in 100 parts of 10% hydrofluoric acid aqueous solution by mass for 20 minutes, and the solid-liquid separation is carried out; the solid is placed in a 300°C oven and baked for 60 minutes; then 50 parts of silicon micropowder are placed in 100 parts of tartaric acid solution with a mass concentration of 2% silver nitrate and heated to 80°C, and 5 parts of citric acid are added, and the reaction is stirred for 120 minutes; solid-liquid separation is carried out, the solid is placed and nitrogen and hydrogen gas flows are passed through it in turn at 600°C, the reduction reaction is carried out for 60 minutes, and the silver-loaded silicon micropowder is obtained.
[0015] By adopting the above technical solution, the silicon micropowder is soaked in a hydrofluoric acid aqueous solution, then baked in an oven, reacted with a tartaric acid solution of silver nitrate, and finally reduced by a nitrogen and hydrogen gas flow to obtain silver-loaded silicon micropowder. In the paper core, the silver-loaded silicon micropowder can improve the antibacterial properties of the material, prevent mildew caused by a humid environment, and maintain the quality and stability of the paper core. At the same time, due to its green and environmentally friendly characteristics, it also meets the green, environmentally friendly and safe requirements of this application.
[0016] Preferably, the preparation method of the hypotonic agent is as follows: after uniformly mixing 50 parts of corn starch and 200 parts of water according to weight proportions, heating to 70°C, reacting for 50 minutes, then heating to 86°C and reacting for 20 minutes, adding 30 parts of trifluoroethyl acrylate, 13 parts of methyl methacrylate, and 4 parts of sodium bicarbonate thereto, and keeping the mixture warm for 4 hours to obtain the hypotonic agent.
[0017] By adopting the above technical scheme, 50 parts of corn starch and 200 parts of water are mixed evenly, heated to 70°C, and reacted for 50 minutes. This step helps the gelatinization of corn starch and fully expands the starch granules. Then the temperature is raised to 86°C for 20 minutes. This step may be intended to further promote the internal structural changes of starch granules, making them easier for subsequent chemical modification. 30 parts of trifluoroethyl acrylate, 13 parts of methyl methacrylate, and 4 parts of sodium bicarbonate are added thereto, and the reaction is kept warm for 4 hours. Corn starch undergoes graft copolymerization with trifluoroethyl acrylate and methyl methacrylate. These monomers have extremely low surface energy and can effectively reduce the surface energy of corn starch on the surface of kraft paper. Finally, a hypopermeability agent is obtained. This modified corn starch can effectively prevent the glue from excessively penetrating into the paper in the antibacterial flame retardant glue, thereby accelerating the drying speed of the glue and significantly improving the bonding strength of the glue.
[0018] Preferably, the preservative is sodium benzoate.
[0019] In a second aspect, the present application provides a method for preparing a paper core with high outer layer flexibility and high inner layer hardness, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned paper core with high outer layer flexibility and high inner layer hardness, comprising the following steps: S91. Evenly stir the modified corn starch, phenolic resin, flame retardant, antibacterial agent, urethane acrylate, hypotonic agent, preservative and water according to their weight proportions to obtain an antibacterial flame retardant glue; S92, selecting hard kraft paper of a specified thickness as a raw material, and rolling to form a hard kraft paper layer paper core; S93. Evenly apply antibacterial and flame-retardant glue on the outer surface of the hard kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard kraft paper core to make them tightly combined through a bonding process. Then, roll the soft kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 85°C for 30-40 minutes to obtain a paper core with a moisture content of 6%-7% and high flexibility of the outer layer and high hardness of the inner layer.
[0020] In summary, the beneficial technical effects of this application are: 1. High bonding strength: A specially formulated antibacterial and flame-retardant glue is used, which optimizes the bonding performance through modified corn starch, phenolic resin and other ingredients to ensure a strong bond between the foam paper layer and the hard kraft paper layer.
[0021] 2. Excellent flame retardant and antibacterial properties: The silver-loaded silica micropowder antibacterial agent and modified bentonite flame retardant added to the antibacterial flame retardant glue provide excellent flame retardant and antibacterial functions, enabling the paper core to form a protective layer and inhibit bacterial growth when encountering fire.
[0022] 3. High radial pressure bearing capacity: Through the combination of hard kraft paper layer and foam paper layer, and the bonding strengthened by glue, the paper core can withstand higher radial pressure.
[0023] 4. Low moisture content 6-7%: This means the paper core has good moisture resistance, maintains the stability and strength of the structure, and extends its service life.
[0024] 5. Green and environmentally friendly: The selected materials such as modified corn starch and hypotonic agents are environmentally friendly materials, easy to degrade, and reduce the negative impact on the environment during the production process.
[0025] 6. Fast drying speed and improved efficiency: The application of low-penetration agent effectively prevents glue from penetrating into the paper, thereby speeding up the drying speed of the glue and improving the efficiency of the production line.
[0026] 7. High safety: Antibacterial flame retardant glue is not only environmentally friendly, but also ensures the safety of the final product during use, especially for applications that require flame retardant and antibacterial properties.
[0027] 8. Balance between flexibility and hardness: The combination of the outer soft kraft paper and the inner hard kraft paper, plus the glue layer and foam layer in the middle, achieves the structural characteristics of soft outside and hard inside, which can meet different usage requirements. DETAILED DESCRIPTION
[0028] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0029] In the following examples and preparation examples, 1 part means 100 g.
[0030] Preparation Example 1 Preparation of modified corn starch The preparation method of modified corn starch comprises the following steps: S31, according to the mass fraction, dissolve 10 parts of corn starch in 30 parts of deionized water, stir evenly, heat to 40°C, stir while heating, stir for 40 minutes, continue to heat to 48°C, keep for 25 minutes, cool to room temperature, and obtain a mixed solution; S32. Add 0.5 parts of 3-chloro-2-hydroxypropyl-trimethylammonium chloride to the mixed solution according to the mass fraction, stir evenly, microwave the mixed substance for 3 minutes, centrifuge and vacuum dry at 80° C. for 24 hours to obtain modified corn starch.
[0031] Preparation Example 2 Preparation of flame retardant The preparation method of the flame retardant comprises the following steps: S41, placing bentonite in a ball mill, ball milling at 400 rpm for 2 h and passing through a 100 mesh sieve; then placing in a muffle furnace, preheating at 260° C. for 35 min, heating to 1020° C., calcining for 2.5 h, and cooling to room temperature to obtain activated bentonite; S42, according to the mass fractions, 100 parts of activated bentonite and 200 parts of sodium hydroxide aqueous solution with a mass concentration of 12% were mixed and allowed to stand for 4 hours; heated to 85° C. and stirred for reaction for 6 hours; cooled, filtered, and the filter residue was collected; the filter residue was washed with water until the pH value of the filtrate was 7, and dried at 105° C. for 12 hours to obtain microporous bentonite; S43, dissolving 100 parts of microporous bentonite and 20 parts of soy protein in 1200 parts of water according to their weight, stirring and reacting at 3000 rpm for 15 hours; filtering, collecting the filter residue, and drying the filter residue at 105° C. for 10 hours to obtain soy protein modified microporous bentonite; S44. Disperse 100 parts of soy protein modified microporous bentonite, 15 parts of sodium alginate and 200 parts of 2-carboxyethylphenyl hypophosphorous acid in water according to their mass proportions, and add the dispersed mixture into a ball mill at a rotor speed of 3000 rpm. Mill the mixture at room temperature for 4 h, centrifuge the mixture at 35000 rpm for 20 min, collect the precipitate, and then dry the precipitate at 85°C for 7 h to obtain a flame retardant.
[0032] Preparation Example 3 Preparation of silver-loaded silicon micropowder The preparation method of silver-loaded silicon micropowder is as follows: according to the mass parts, 50 parts of silicon micropowder are soaked in 100 parts of 10% hydrofluoric acid aqueous solution by mass for 20 minutes, and the solid-liquid separation is carried out; the solid is placed in a 300°C oven and baked for 60 minutes; then 50 parts of silicon micropowder are placed in 100 parts of tartaric acid solution with a mass concentration of 2% silver nitrate and heated to 80°C, and then 5 parts of citric acid are added, and the reaction is stirred for 120 minutes; solid-liquid separation is carried out, the solid is placed and nitrogen and hydrogen gas flows are passed through it in turn at 600°C, the reduction reaction is carried out for 60 minutes, and it is cooled to room temperature to obtain silver-loaded silicon micropowder.
[0033] Preparation Example 4 Preparation of hypotonic agent The preparation method of the hypotonic agent is as follows: 50 parts of corn starch and 200 parts of water are mixed evenly according to their weight proportions, heated to 70°C, reacted for 50 minutes, then heated to 86°C for reaction for 20 minutes, 30 parts of trifluoroethyl acrylate, 13 parts of methyl methacrylate, and 4 parts of sodium bicarbonate are added thereto, and after heat preservation and reaction for 4 hours, the hypotonic agent is obtained.
[0034] Preparation Comparative Example 1 Same as Preparation Example 4, except that the added amount of trifluoroethyl acrylate was 0 parts and the added amount of methyl methacrylate was 43 parts.
[0035] Example 1 A paper core with high flexibility in the outer layer and high hardness in the inner layer, which comprises, from the inside to the outside, a hard kraft paper layer, an antibacterial flame retardant glue layer, a foam paper layer and a soft kraft paper layer, wherein the antibacterial flame retardant glue layer is prepared by coating the antibacterial flame retardant glue on the surface of the hard kraft paper layer and bonding the foam paper layer, wherein the antibacterial flame retardant glue comprises the following preparation raw materials by mass: 60 parts of modified corn starch, 3 parts of phenolic resin, 5 parts of flame retardant, 3 parts of silver-loaded silicon micropowder, 0.3 parts of urethane acrylate, 0.2 parts of hypotonic agent, 0.3 parts of preservative, and 300 parts of water; the inner diameter of the paper core is 77 mm, the thickness is 5 mm, the thickness of the hard kraft paper layer is 0.5 mm, the soft kraft paper layer is 0.5 mm, and the foam paper layer is 4 mm.
[0036] The method for preparing the paper core having high outer layer flexibility and high inner layer hardness comprises the following steps: S91. Evenly stir the modified corn starch, phenolic resin, flame retardant, silver-loaded silica powder, urethane acrylate, hypotonic agent, sodium benzoate and water according to their weight proportions to obtain an antibacterial flame retardant glue; S92, selecting hard kraft paper of a specified thickness as a raw material, and rolling to form a hard kraft paper layer paper core; S93. Evenly apply antibacterial and flame-retardant glue on the outer surface of the hard kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard kraft paper core to make them tightly combined through a bonding process. Then, roll the soft kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 85°C for 30 minutes to obtain a paper core with a moisture content of 7% and a high outer layer flexibility and a high inner layer hardness.
[0037] Example 2 A paper core with high flexibility in the outer layer and high hardness in the inner layer, which comprises, from the inside to the outside, a hard kraft paper layer, an antibacterial flame retardant glue layer, a foam paper layer and a soft kraft paper layer, wherein the antibacterial flame retardant glue layer is prepared by coating the antibacterial flame retardant glue on the surface of the hard kraft paper layer and bonding the foam paper layer, wherein the antibacterial flame retardant glue comprises the following preparation raw materials by mass: 70 parts of modified corn starch, 5 parts of phenolic resin, 7 parts of flame retardant, 4 parts of silver-loaded silicon micropowder, 0.5 parts of amino acrylate, 0.3 parts of hypotonic agent, 0.4 parts of preservative, and 330 parts of water; the inner diameter of the paper core is 80 mm, the thickness is 6 mm, the thickness of the hard kraft paper layer is 1 mm, the soft kraft paper layer is 1 mm, and the foam paper layer is 4 mm.
[0038] The method for preparing the paper core having high outer layer flexibility and high inner layer hardness comprises the following steps: S91. Evenly stir the modified corn starch, phenolic resin, flame retardant, silver-loaded silica powder, urethane acrylate, hypotonic agent, sodium benzoate and water according to their weight proportions to obtain an antibacterial flame retardant glue; S92, selecting hard kraft paper of a specified thickness as a raw material, and rolling to form a hard kraft paper layer paper core; S93. Evenly apply antibacterial and flame-retardant glue on the outer surface of the hard kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard kraft paper core to make them tightly combined through a bonding process. Then, roll the soft kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 85°C for 40 minutes to obtain a paper core with a moisture content of 6% and a high outer layer flexibility and a high inner layer hardness.
[0039] Example 3 A paper core with high flexibility in the outer layer and high hardness in the inner layer, which comprises, from the inside to the outside, a hard kraft paper layer, an antibacterial flame retardant glue layer, a foam paper layer and a soft kraft paper layer, wherein the antibacterial flame retardant glue layer is prepared by coating the antibacterial flame retardant glue on the surface of the hard kraft paper layer and bonding the foam paper layer, wherein the antibacterial flame retardant glue comprises the following preparation raw materials by mass: 66 parts of modified corn starch, 4 parts of phenolic resin, 6 parts of flame retardant, 3.5 parts of silver-loaded silicon micropowder, 0.4 parts of urethane acrylate, 0.25 parts of hypotonic agent, 0.35 parts of preservative, and 315 parts of water; the inner diameter of the paper core is 78 mm, the thickness is 5.5 mm, the thickness of the hard kraft paper layer is 0.5 mm, the soft kraft paper layer is 0.5 mm, and the foam paper layer is 4.5 mm.
[0040] The method for preparing the paper core having high outer layer flexibility and high inner layer hardness comprises the following steps: S91. Evenly stir the modified corn starch, phenolic resin, flame retardant, silver-loaded silica powder, urethane acrylate, hypotonic agent, sodium benzoate and water according to their weight proportions to obtain an antibacterial flame retardant glue; S92, selecting hard kraft paper of a specified thickness as a raw material, and rolling to form a hard kraft paper layer paper core; S93. Evenly apply antibacterial and flame-retardant glue on the outer surface of the hard kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard kraft paper core to make them tightly combined through a bonding process. Then, roll the soft kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 85°C for 36 minutes to obtain a paper core with a moisture content of 6.6% and high flexibility of the outer layer and high hardness of the inner layer.
[0041] Comparative Example 1 The same as Example 3, except that an equal amount of corn starch is used instead of modified corn starch.
[0042] Comparative Example 2 The same as Example 3, except that an equal amount of 2-carboxyethylphenylphosphite is used instead of the flame retardant.
[0043] Comparative Example 3 The same as Example 3, except that an equal amount of the hypotonic agent prepared in Comparative Preparation Example 1 is used instead of the hypotonic agent prepared in Preparation Example 4.
[0044] Performance Testing 1. The paper cores with high outer flexibility and high inner hardness obtained in Examples 1 to 3 were sampled and tested as follows. The test results are shown in Table 1.
[0045] Moisture content, radial compression resistance: tested in accordance with BB / T0032-2006 standard.
[0046] 2. The antibacterial flame retardant glue prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was sampled, and the antibacterial flame retardant glue was coated on the glass surface and dried to obtain strips with a thickness of 2 mm to test the antibacterial and flame retardant properties, and the following tests were performed. The test results are shown in Table 2.
[0047] Adhesion strength test: Tested using the method described in GB / T6541-2011; The antibacterial rate is tested according to JIS Z2801:2000 standard; Flame retardancy test: Place the sample to be tested in a glass combustion tube, introduce a nitrogen-oxygen mixed gas flow, record the minimum oxygen concentration required for combustion, and take the average value of five tests for each group; Permeability determination: Press the PVC sheet with rectangular holes on the paper, and fill the groove glue area with a pencil as the initial glue area, which is recorded as the control sample. Use a camera to take pictures of the paper sample coated with antibacterial flame retardant glue and the control sample that have been naturally cured. Use the pixel method to import the picture into Photoshop software, set the feather value to 0, remove the anti-aliasing option, and use the magnetic lasso tool to select the blue antibacterial flame retardant glue area in the tipping paper. Keep the ant line floating, select "Window"-"Histogram" command, and the histogram dialog box pops up. Read out the number of pixels contained in the selection, which is recorded as the number of pixels in the glue area after the antibacterial flame retardant glue is cured. The control sample is treated in the same way, and the number of pixels in the initial glue area is recorded; Permeability calculation: subtract the number of pixels in the initial glue coating area from the number of pixels in the glue area after the antibacterial flame retardant glue is cured, and the ratio of the number of pixels in the penetration area to the number of pixels in the initial glue coating area is the permeability k of the antibacterial flame retardant glue. The permeability of antibacterial flame retardant glue is calculated according to the following formula: k = (N2-N1) / N1, where k is the permeability of antibacterial flame retardant glue, N2 is the pixel value after the antibacterial flame retardant glue is cured, and N1 is the pixel value of the initial glue coating area.
[0048] Table 1 Paper core performance test project Moisture content / % Radial compression resistance / N Example 1 7 1338 Example 2 6 1423 Example 3 6.6 1385 Table 2 Antibacterial flame retardant glue performance test Analyzing the data in Tables 1 and 2, we can see that: 1) The paper core with high outer layer flexibility and high inner layer hardness prepared in Examples 1 to 3 has high radial pressure, is green, environmentally friendly and safe, and has low moisture content (6-7%). The antibacterial flame retardant glue prepared in this application has the advantages of excellent antibacterial properties, flame retardancy, low permeability and high bonding strength, and is also highly safe and environmentally friendly.
[0049] 2) The performance comparison analysis of the antibacterial flame retardant glue prepared in combination with Example 3 and Comparative Example 1 shows that the modified corn starch increases the compatibility with the resin, especially the compatibility with the phenolic resin, by grafting 3-chloro-2-hydroxypropyl-trimethylammonium chloride. This helps to improve the overall performance of the antibacterial flame retardant glue, ensure good interaction between the components, and thus improve the bonding strength and durability of the paper core. As one of the main ingredients in the antibacterial flame retardant glue, the modified corn starch has excellent bonding properties that help to firmly bond the foam paper layer to the hard kraft paper layer, while providing the required flexibility and hardness for the paper core. Modified corn starch is a renewable resource, and its use conforms to the principle of green environmental protection. In addition, the modified corn starch itself is biodegradable and will not cause long-term pollution to the environment. The combination of modified corn starch and hypotonic agent (corn starch graft copolymer) can effectively prevent the antibacterial flame retardant glue from excessive penetration inside the paper, which not only speeds up the drying speed of the antibacterial flame retardant glue, but also improves the bonding strength and ensures the overall performance of the paper core.
[0050] 3) The performance comparison analysis of the antibacterial flame retardant glue prepared in combination with Example 3 and Comparative Example 2 shows that the flame retardant prepared in this application includes the activation of bentonite, the preparation of microporous bentonite, the modification of soy protein and the synthesis of the final composite flame retardant. These steps are intended to improve the dispersibility and flame retardant properties of bentonite, and further enhance its flame retardant effect by adding sodium alginate and 2-carboxyethylphenyl hypophosphite. The addition of sodium alginate and 2-carboxyethylphenyl hypophosphite, together with bentonite and soy protein, forms an efficient flame retardant system, which not only improves the flame retardancy, but also increases the smoke density and char strength of the material.
[0051] 4) The performance comparison analysis of the antibacterial flame retardant glue prepared in Example 3 and Comparative Example 3 shows that the low permeability agent prepared in the present application, by grafting and copolymerizing corn starch with trifluoroethyl acrylate and methyl methacrylate, these monomers have extremely low surface energy and can effectively reduce the surface energy of corn starch on the surface of kraft paper. The modified corn starch in the antibacterial flame retardant glue can effectively prevent the glue from excessively penetrating into the paper, thereby accelerating the drying speed of the glue and significantly improving the bonding strength of the glue.
[0052] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.
Claims
1. A paper core with high outer layer flexibility and high inner layer hardness, characterized in that: From the inside to the outside, it includes a hard kraft paper layer, an antibacterial flame retardant glue layer, a foam paper layer and a soft kraft paper layer. The antibacterial flame retardant glue layer is prepared by coating the antibacterial flame retardant glue on the surface of the hard kraft paper layer and bonding the foam paper layer. The antibacterial flame retardant glue includes the following raw materials by mass: 60-70 parts of modified corn starch, 3-5 parts of phenolic resin, 5-7 parts of flame retardant, 3-4 parts of antibacterial agent, 0.3-0.5 parts of urethane acrylate, 0.2-0.3 parts of hypotonic agent, 0.3-0.4 parts of preservative and 300-330 parts of water.
2. A paper core with high outer layer flexibility and high inner layer hardness according to claim 1, characterized in that: The inner diameter of the paper core is 77-80 mm, the thickness is 5-6 mm, the thickness of the hard kraft paper layer is 0.5-1 mm, the thickness of the soft kraft paper layer is 0.5-1 mm, and the thickness of the foam paper layer is 4-5 mm.
3. A paper core with high outer layer flexibility and high inner layer hardness according to claim 1, characterized in that: The preparation method of the modified corn starch comprises the following steps: S31, according to the mass fraction, dissolve 10 parts of corn starch in 30 parts of deionized water, stir evenly, heat to 40°C, stir while heating, stir for 40 minutes, continue to heat to 48°C, keep for 25 minutes, cool to room temperature, and obtain a mixed solution; S32. Add 0.5 parts of 3-chloro-2-hydroxypropyl-trimethylammonium chloride to the mixed solution according to the mass fraction, stir evenly, microwave the mixed substance for 3 minutes, centrifuge and vacuum dry at 80° C. for 24 hours to obtain modified corn starch.
4. A paper core with high outer layer flexibility and high inner layer hardness according to claim 1, characterized in that: The method for preparing the flame retardant comprises the following steps: S41, placing bentonite in a ball mill, ball milling at 400 rpm for 2 h and passing through a 100 mesh sieve; then placing in a muffle furnace, preheating at 260° C. for 35 min, heating to 1020° C., calcining for 2.5 h, and cooling to room temperature to obtain activated bentonite; S42, according to the mass fractions, 100 parts of activated bentonite and 200 parts of sodium hydroxide aqueous solution with a mass concentration of 12% were mixed and allowed to stand for 4 hours; heated to 85°C, stirred and reacted for 6 hours; cooled, filtered, and the filter residue was collected; the filter residue was washed with water until the pH value of the filtrate was 7, and dried at 105°C for 12 hours to obtain microporous bentonite; S43, dissolving 100 parts of microporous bentonite and 20 parts of soy protein in 1200 parts of water according to their weight, stirring and reacting at 3000 rpm for 15 hours; filtering, collecting the filter residue, and drying the filter residue at 105° C. for 10 hours to obtain soy protein modified microporous bentonite; S44. Disperse 100 parts of soy protein modified microporous bentonite, 15 parts of sodium alginate and 200 parts of 2-carboxyethylphenyl hypophosphorous acid in water according to their mass proportions, and add the dispersed mixture into a ball mill at a rotor speed of 3000 rpm. Mill the mixture at room temperature for 4 h, centrifuge the mixture at 35000 rpm for 20 min, collect the precipitate, and then dry the precipitate at 85°C for 7 h to obtain a flame retardant.
5. The paper core according to claim 1, wherein the outer layer has high flexibility and the inner layer has high hardness, The antibacterial agent is silver-loaded silicon powder.
6. A paper core with high outer layer flexibility and high inner layer hardness according to claim 5, characterized in that: The preparation method of the silver-loaded silicon micropowder is as follows: according to the mass fraction, 50 parts of silicon micropowder are soaked in 100 parts of hydrofluoric acid aqueous solution with a mass concentration of 10% for 20 minutes, solid-liquid separation is performed, and the solid is placed in a 300° C. oven for baking for 60 minutes; then 50 parts of silicon micropowder are placed in 100 parts of tartaric acid solution with a mass concentration of 2% silver nitrate, heated to 80° C., 5 parts of citric acid are added, and stirred for reaction for 120 minutes; solid-liquid separation is performed, the solid is placed and nitrogen and hydrogen gas flows are passed through it in turn at 600° C., reduction reaction is performed for 60 minutes, and cooling is performed to room temperature to obtain the silver-loaded silicon micropowder.
7. A paper core with high outer layer flexibility and high inner layer hardness according to claim 1, characterized in that: The preparation method of the hypotonic agent is as follows: 50 parts of corn starch and 200 parts of water are mixed uniformly according to weight proportions, heated to 70° C., reacted for 50 minutes, then heated to 86° C., reacted for 20 minutes, 30 parts of trifluoroethyl acrylate, 13 parts of methyl methacrylate, and 4 parts of sodium bicarbonate are added thereto, and the mixture is kept warm for reaction for 4 hours to obtain the hypotonic agent.
8. The paper core according to claim 1, characterized in that: The preservative is sodium benzoate.
9. A method for preparing a paper core with high outer layer flexibility and high inner layer hardness as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: S91. Evenly stir the modified corn starch, phenolic resin, flame retardant, antibacterial agent, urethane acrylate, hypotonic agent, preservative and water according to their weight proportions to obtain an antibacterial flame retardant glue; S92, selecting hard kraft paper of a specified thickness as a raw material, and rolling to form a hard kraft paper layer paper core; S93. Evenly apply antibacterial and flame-retardant glue on the outer surface of the hard kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard kraft paper core to make them tightly combined through the bonding process. Then, roll the soft kraft paper layer on the outer layer of the foam paper again, and dry it at 85°C for 30-40 minutes to obtain a paper core with a moisture content of 6%-7% and high flexibility of the outer layer and high hardness of the inner layer.
Citation Information
Patent Citations
Low-permeability paper mounting glue and preparation method thereof
CN111117520A
Fruit fresh-keeping bactericide as well as preparation method and application thereof
CN111802453A
Composite material for high-strength corrugated board and preparation method of composite material
CN115384164A
Glue for paper products and preparation method thereof
CN116515420A
Environment-friendly seamless paper tube and processing method thereof
CN117507493A