Energy storage battery with quick charge and discharge capability

By using the combination of negative electrode materials of Nb2O5 and activated carbon and the positive electrode materials of Nb-LiMn2O4 particles containing niobium, combined with specific adhesives and conductive additives, the electrical performance of the supercapacitor is optimized, and the problems of large voltage changes and insufficient cycle stability are solved. High peak power and higher energy density are achieved.

CN119069264APending Publication Date: 2024-12-03SKELETON TECH GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410707614.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-06-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The current supercapacitors have large voltage changes during charging and discharging, making it difficult to meet the needs of high peak power applications. At the same time, the cycle stability of lithium manganese oxide batteries is insufficient, resulting in capacity loss.

Method used

The electrode is prepared by slurry coating and heating using a negative electrode active material composition composed of Nb2O5 particles and activated carbon and a positive electrode active material composed of Nb-LiMn2O4 particles containing niobium, combined with specific binders and conductive additives, and the electrode is prepared by slurry coating and heating, and using organic non-free Water electrolyte, optimize battery structure and components.

Benefits of technology

Improves the charging/discharge speed and cycling stability of the energy storage battery, reduces the equivalent series resistance, enhances the available capacity and voltage, and achieves higher energy and power density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004873089920000061
    Figure BDA0004873089920000061
  • Figure BDA0004873089920000071
    Figure BDA0004873089920000071
Patent Text Reader

Abstract

An energy storage cell for storing electrical energy, the energy storage cell comprising a negative electrode and a positive electrode immersed in an organic anhydrous electrolyte, where the negative electrode comprises a negative active material composition having Nb2O5 particles and activated carbon (AC) particles; wherein the positive electrode includes a positive electrode active material composition, the majority of which has LiMn2O4 (LMO) particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to energy storage cells (eg, hybrid supercapacitors) and components thereof (eg, electrodes and electrolytes) having rapid charge and discharge capabilities. Background Art

[0002] Whether in the automotive, industrial applications, public transport or grid regulation sectors, the demand for energy storage batteries has increased significantly in recent years. These batteries can be used as traction batteries, intermediate energy storage for kinetic energy recovery systems or energy storage for mechanical assistance systems (such as anti-skid systems or active shock absorbers). In grid regulation, batteries store excess production energy (especially excess wind or solar energy) and help to fill energy gaps in cases of high demand. For all these applications, it is useful to have an energy storage battery that allows fast charging or discharging or, in other words, high peak powers.

[0003] Energy storage cells can generally be divided into batteries and capacitors. Batteries store electrical energy in a chemical form, while capacitors usually store electrical energy in the form of an electric field. Batteries are generally not able to achieve the peak power required for the above applications.

[0004] Ultracapacitors, also known as supercapacitors, are a type of capacitor and can be divided into double-layer capacitors and pseudocapacitors. The former stores electrical energy in an electrostatic double layer, while the latter stores electrical energy electrochemically, but in a different way than batteries. Recently, hybrid (super)capacitors have been developed that combine the features of double-layer capacitors and pseudocapacitors.

[0005] These capacitors typically exhibit large voltage changes during charge and discharge, whereas batteries do not. The main advantage of capacitors is that they are well suited for applications that require large peak powers, or in other words, applications that require the transfer of large amounts of energy in a very short period of time.

[0006] This capability (especially for supercapacitors) is not unlimited, since usually the actually usable capacity depends on the discharge current: the higher the current, the lower the usable capacity.

[0007] Among the materials used in lithium batteries at the positive electrode, lithium manganese oxide (LMO) has recently gained considerable attention (especially for high-rate applications), partly due to the safety of production equipment. However, one drawback to the long-life cycling stability of these batteries is the dissolution of manganese ions into the electrolyte, resulting in capacity loss.

[0008] US5258245A discloses a lithium battery comprising a positive electrode mainly composed of vanadium pentoxide, a negative electrode mainly composed of niobium pentoxide doped with lithium, and an electrolyte mainly composed of an anhydrous solvent in which a lithium salt is dissolved.

[0009] US2021 / 0110980A1, US2021 / 0110979A1 and US2021 / 0218048A1 disclose battery concepts using three or four electrodes.

[0010] DE 10 2018 202 929 A1 discloses a hybrid supercapacitor. Summary of the invention

[0011] The object of the present invention is to improve the electrical performance of supercapacitors, preferably to improve the practically available capacity or the charge / discharge rate. Another object of the present invention is to use niobium-containing lithium manganese oxide as a positive electrode active material to improve the cycle stability.

[0012] The present invention provides a negative electrode active material composition for a negative electrode of an energy storage battery, the composition comprising the following components:

[0013] -70wt% to 99wt% of negative electrode active material;

[0014] - 1 to 10 wt % of at least one binder;

[0015] - optionally, a total amount of up to 10 wt% of at least one conductive additive; and

[0016] -optionally, other components or impurities in a total amount less than 10 wt%,

[0017] Wherein, the negative electrode active material is Nb 2 O 5 particles and activated carbon (AC) particles.

[0018] The present invention provides a method for manufacturing a negative electrode for an energy storage battery, the method comprising:

[0019] a) providing 1 wt% to 20 wt% of a binder in a mixing container;

[0020] b) mixing the following materials in the container to obtain a slurry:

[0021] -60wt% to 99wt% of a negative electrode active material, the negative electrode active material comprising 1wt% to 99wt% of Nb 2 O 5 particles and a balance of up to 100 wt % of activated carbon (AC) particles;

[0022] - optionally, a total amount of up to 10 wt% of at least one conductive additive; and

[0023] - Optionally, other components in a total amount less than 10 wt%;

[0024] c) coating a conductive electrode substrate with the slurry, and heating the coated electrode substrate, thereby producing the negative electrode.

[0025] In the embodiment, the total proportion of all binders is 2wt% to 4wt%, and the proportion of negative electrode active material is 76wt% to 98wt%. In the embodiment, the proportion of each binder does not exceed 2wt%.

[0026] In an embodiment, Nb 2 O 5 The content of the particles is 30wt%, 40wt%, 50wt%, 60wt% or 70wt%. In an embodiment, the content of the AC particles is 30wt%, 40wt%, 50wt%, 60wt% or 70wt%.

[0027] In an embodiment, the negative electrode active material is composed of Nb 2 O 5 In the embodiment, Nb 2 O 5 The particles are mainly composed of orthorombic Nb 2 O 5 In the embodiment, Nb 2 O 5 The particles consist of more than 90 wt% orthorhombic Nb 2 O 5 composition.

[0028] In an embodiment, Nb 2 O 5 The particle size D90 of the particles is 1 μm to 100 μm, preferably 2 μm to 60 μm, more preferably 10 μm to 30 μm. 2 O 5 The particle size D10 of the particles is 0.05 μm to 10 μm, preferably 0.3 μm to 5 μm, and more preferably 0.3 μm to 3 μm.

[0029] In an embodiment, the AC particles have a diameter of at least 60 μm. 2 / g, preferably at least 1000m 2 / g of BET nitrogen surface area.

[0030] In an embodiment, the AC particles have a particle size D90 of 5 to 30 μm, preferably 5 to 20 μm. In an embodiment, the AC particles have a particle size D10 of 1 to 2 μm. In an embodiment, the AC particles include carbide derived carbon (CDC) particles.

[0031] In an embodiment, each conductive additive is selected from the group consisting of carbon black, carbon nanotubes (CNTs), graphene, and mixtures thereof. Preferably, the CNTs are multi-walled CNTs (MWCNTs).

[0032] In an embodiment, the composition comprises 1 wt% to 10 wt% carbon black. In an embodiment, the composition comprises 1 wt% to 8 wt% carbon black. In an embodiment, the composition comprises 1 wt% to 3 wt% carbon black. In an embodiment, the composition comprises 2 wt% to 6 wt% carbon black. In an embodiment, the composition comprises 3 wt% to 7 wt% carbon black.

[0033] In embodiments, the composition comprises 0.3 wt% to 2 wt% CNTs. In embodiments, the composition comprises 0.3 wt% to 1.0 wt% CNTs.

[0034] The present invention provides a positive electrode active material composition for a positive electrode of an energy storage battery, the composition comprising the following components:

[0035] - 0.5 to 10 wt% of carbon black (CB);

[0036] - 1 wt% to 20 wt% of at least one binder;

[0037] -56 wt% to 98.5 wt% of a positive electrode active material, the positive electrode active material mostly comprising or mostly consisting of Nb-LiMn containing niobium 2 O 4 (Nb-LMO) particles, wherein the content of niobium in the positive electrode active material is optionally between 0.001wt% and 5.0wt% based on the mass of lithium manganese oxide;

[0038] - Optionally, 0.1 wt% to 2 wt% of carbon nanotubes (CNTs);

[0039] - optionally, 0.1 wt% to 2 wt% of graphene; and

[0040] - Optionally, less than 10 wt% of other components or impurities.

[0041] The present invention provides a method for manufacturing a positive electrode for an energy storage battery, the method comprising:

[0042] a) providing 1 wt% to 20 wt% of a binder in a mixing container;

[0043] b) mixing the following materials in the container to obtain a slurry:

[0044] - 0.5 to 10 wt% of carbon black (CB);

[0045] -56wt% to 98.5wt% of Nb-LiMn 2 O 4 A positive electrode active material composed of (Nb-LMO) particles;

[0046] - Optionally, 0.1 wt% to 2 wt% of carbon nanotubes (CNTs); and

[0047] - Optionally, 0.1 wt% to 2 wt% of graphene;

[0048] c) coating a conductive electrode substrate with the slurry, and heating the coated electrode substrate, thereby producing the positive electrode.

[0049] In an embodiment, the particle size D90 of the Nb-LMO particles is 30 μm to 40 μm. Preferably, the particle size D50 of the Nb-LMO particles is 10 μm to 20 μm. Preferably, the particle size D10 of the Nb-LMO particles is 3 μm to 9 μm.

[0050] In an embodiment, the proportion of CNTs deviates from the proportion of graphene by less than 10%, and vice versa. In an embodiment, the proportions of CNTs and graphene are the same.

[0051] The present invention provides an energy storage battery for storing electrical energy, the battery comprising a plurality of electrodes immersed in an organic anhydrous electrolyte, wherein at least one electrode is configured as a negative electrode, and at least one electrode is configured as a positive electrode, wherein the negative electrode comprises the negative electrode material composition as described above or the negative electrode material composition obtainable by the aforementioned method. Alternatively or additionally, the positive electrode comprises the positive electrode material composition as described above or the positive electrode material composition obtainable by the aforementioned method.

[0052] In an embodiment, the electrolyte consists of 80 vol% to 95 vol% of acetonitrile, 5 vol% to 20 vol% of ethylene carbonate and a lithium conductive salt.

[0053] The present invention provides an organic anhydrous electrolyte composition for energy storage batteries, the composition consisting of:

[0054] - 80 vol% to 95 vol% acetonitrile;

[0055] -5vol% to 20vol% of ethylene carbonate; in addition

[0056] - Lithium conductive salts.

[0057] In the embodiment, the proportion of acetonitrile is 85vol% to 93vol%, and the proportion of ethylene carbonate is 7vol% to 15vol%. In the embodiment, the proportion of acetonitrile is 88vol% to 93vol%, and the proportion of ethylene carbonate is 7vol% to 12vol%. In the embodiment, the proportion of acetonitrile is 89vol% to 91vol%, and the proportion of ethylene carbonate is 9vol% to 11vol%.

[0058] In an embodiment, the concentration of the conductive lithium salt is 0.1 mol / L to 3 mol / L.

[0059] In an embodiment, the lithium conductive salt is selected from lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4 ), lithium hexafluorophosphate (LiPF 6 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium trifluoromethanesulfonate (LiSO 3 CF 3 ), lithium bis(trifluoromethylsulfonyl)imide (LiN(SO 2 CF 3 ) 2 ), lithium bis(pentafluoroethanesulfonyl)imide (LiN(SO 2 C 2 F 5 ) 2 ), lithium bis(oxalate)borate (LiBOB, LiB(C 2 O 4 ) 2 ), lithium difluoro(oxalato)borate (LiBF 2 (C 2 O 4 )), lithium tris(pentafluoroethyl) trifluorophosphate (LiPF 3 (C 2 F 5 ) 3 ) and mixtures thereof. In an embodiment, the lithium conductive salt is LiPF 6 .

[0060] The present invention provides an energy storage battery for storing electric energy, the battery comprising a positive electrode and a negative electrode immersed in an organic anhydrous electrolyte,

[0061] Wherein, the negative electrode comprises Nb 2 O 5 Negative electrode active material composition of particles and activated carbon (AC) particles;

[0062] Wherein, the positive electrode comprises a positive electrode active material composition, wherein the positive electrode active material composition has a majority of Nb-LiMn 2 O 4 (Nb-LMO) particles.

[0063] In an embodiment, the negative electrode active material composition includes Nb 2 O 5 The negative electrode active material consists of particles and AC particles.

[0064] In an embodiment, Nb 2 O 5 The content of the particles and the content of the AC particles are selected from the group consisting of 30 wt %, 40 wt %, 50 wt %, 60 wt % and 70 wt % such that the total amount is 100 wt %.

[0065] In embodiments, the negative electrode composition and / or the positive electrode composition includes at least one conductive additive.

[0066] In an embodiment, the at least one conductive additive is selected from the group consisting of carbon black (CB), carbon nanotubes (CNT), graphene, and mixtures thereof.

[0067] In an embodiment, the negative electrode active material composition is composed of more than 50wt%, preferably more than 60wt% of the negative electrode active material. In an embodiment, the positive electrode active material composition is composed of more than 50wt%, preferably more than 90wt%, preferably more than 95wt%, preferably more than 97wt% or more of the positive electrode active material.

[0068] In an embodiment, Nb 2 O 5 The particle size D90 of the particles is 1 μm to 100 μm, preferably 2 μm to 60 μm, and more preferably 10 μm to 30 μm. 2 O 5 The particle size D10 of the particles is 0.05 μm to 10 μm, preferably 0.3 μm to 5 μm, and more preferably 0.3 μm to 3 μm.

[0069] In an embodiment, the AC particles have a diameter of at least 60 μm. 2 / g, preferably at least 1000m 2 / g of BET nitrogen surface area.

[0070] In an embodiment, the particle size D90 of the AC particles is 5 μm to 30 μm, preferably 5 μm to 20 μm. In an embodiment, the particle size D10 of the AC particles is 1 μm to 2 μm.

[0071] In embodiments, the AC particles include carbide derived carbon particles.

[0072] In an embodiment, the CNTs are multi-walled CNTs (MWCNTs).

[0073] In an embodiment, the negative electrode composition comprises 1 wt% to 10 wt% carbon black. In an embodiment, the negative electrode composition comprises 1 wt% to 8 wt% carbon black. In an embodiment, the negative electrode composition comprises 1 wt% to 3 wt% carbon black. In an embodiment, the negative electrode composition comprises 2 wt% to 6 wt% carbon black. In an embodiment, the negative electrode composition comprises 3 wt% to 7 wt% carbon black.

[0074] In an embodiment, the positive electrode composition comprises 1 wt% to 10 wt% carbon black. In an embodiment, the positive electrode composition comprises 1 wt% to 8 wt% carbon black. In an embodiment, the positive electrode composition comprises 1 wt% to 3 wt% carbon black. In an embodiment, the positive electrode composition comprises 2 wt% to 6 wt% carbon black. In an embodiment, the positive electrode composition comprises 3 wt% to 7 wt% carbon black.

[0075] In embodiments, the negative electrode composition comprises 0.3 wt% to 2 wt%, preferably 0.3 wt% to 1.0 wt% CNTs. In embodiments, the positive electrode composition comprises 0.3 wt% to 2 wt%, preferably 0.3 wt% to 1.0 wt% CNTs.

[0076] In embodiments, the negative electrode composition comprises 0.3 wt% to 2 wt%, preferably 0.3 wt% to 1.0 wt% graphene. In embodiments, the positive electrode composition comprises 0.3 wt% to 2 wt%, preferably 0.3 wt% to 1.0 wt% graphene.

[0077] In an embodiment, the proportion of CNTs deviates from the proportion of graphene by less than 10%, and vice versa. In an embodiment, the proportions of CNTs and graphene are the same.

[0078] In an embodiment, the electrolyte includes a lithium conductive salt, 80 vol% to 95 vol% acetonitrile, and 5 vol% to 20 vol% ethylene carbonate.

[0079] In an embodiment, the lithium conductive salt is selected from lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4 ), lithium hexafluorophosphate (LiPF 6 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium trifluoromethanesulfonate (LiSO 3 CF 3), lithium bis(trifluoromethylsulfonyl)imide (LiN(SO 2 CF 3 ) 2 ), lithium bis(pentafluoroethanesulfonyl)imide (LiN(SO 2 C 2 F 5 ) 2 ), lithium bis(oxalate)borate (LiBOB, LiB(C 2 O 4 ) 2 ), lithium difluoro(oxalato)borate (LiBF 2 (C 2 O 4 )), lithium tris(pentafluoroethyl) trifluorophosphate (LiPF 3 (C 2 F 5 ) 3 ) and mixtures thereof. In an embodiment, the lithium conductive salt is LiPF 6 .

[0080] Nb 2 O 5 The particles are capable of undergoing redox reactions and inserting lithium ions into their crystal structure. The activated carbon particles include micropores that provide storage space for metallic lithium. Due to the mixing of the two, the path length of lithium to the location where redox reactions can occur during charging or discharging is quite short. As a result, the equivalent series resistance (ESR) can be reduced to less than 1.5mΩ within a 1s (discharge) charging time. For a shorter (discharge) charging time of 10ms, the ESR can be further reduced to less than 0.5mΩ.

[0081] The applicant has experimentally found that a specific composition of the conductive additive allows to increase the available gravimetric capacity in terms of gravimetric current. Gravimetric capacity is the amount of milliampere-hours per gram of active material, whereas gravimetric current is the amount of milliamperes per gram of active material.

[0082] Adding graphene or CNT increases the available weight capacity at a weight current below 400mA / g. Surprisingly, adding equal amounts of CNT and graphene has the best effect (especially for the positive electrode). Herein, for a weight current of up to 1000mA / g, a weight capacity of 80mAh / g to 120mAh / g can be achieved. For a weight current of more than 200mA / g, the maximum gain can be obtained, wherein the available weight capacity is about 2 to 5 times that of an electrode having only one conductive additive.

[0083] Adding CNTs alone to carbon black can triple the usable gravimetric capacity of the negative electrode. For gravimetric currents up to 1000 mA / g, the use of CNTs can result in a usable gravimetric capacity of over 80 mA / g.

[0084] Another improvement of the present invention is the available cell voltage. Considering the sacrificial additives in the electrolyte that passivate the electrodes, the cell voltage of a lithium ion battery (LIB) is about 4.2V. This is undesirable in the present invention because the passivation reduces the available peak power capacity. 2 O 5 ), the cell voltage can reach 3.0 V. The electrolyte composition can be further improved and is stable enough to achieve these voltages.

[0085] The active material of the electrode allows for a higher electrode density, which translates into a higher energy density, at least for supercapacitors. In general, applicants have found that the gravimetric energy density (i.e., the number of Watt-hours per kilogram of active material) can be doubled compared to conventional batteries. Although the gravimetric energy density depends on the gravimetric battery power (i.e., the number of Watts per kilogram of active material), this improvement is independent of the gravimetric battery power. Therefore, an overall improvement in electrical performance can be achieved for a wide range of applications. DETAILED DESCRIPTION

[0086] Energy Storage Batteries

[0087] The energy storage battery can be configured as a hybrid supercapacitor. The energy storage battery is preferably formed as a cylinder. The energy storage battery includes a first electrode device and a second electrode device. Both electrode devices are immersed in an organic anhydrous electrolyte. In addition, the energy storage battery includes a separator disposed between the first electrode device and the second electrode device.

[0088] It should be noted that the energy storage cell generally comprises a plurality of windings of the first electrode arrangement and the second electrode arrangement around the cylindrical axis, however, for the sake of clarity, only some of the windings are shown here.

[0089] The first electrode arrangement comprises a negative terminal. The negative terminal is arranged so that an external electrical contact can be formed. The first electrode arrangement comprises a negative electrode. The negative electrode is electrically coupled to the negative terminal. The negative electrode comprises a current collector made of a metal, preferably aluminum. The current collector contacts the negative terminal. The negative electrode comprises a negative electrode material.

[0090] The second electrode arrangement comprises a positive terminal. The positive terminal is arranged so that an external electrical contact can be made. The second electrode arrangement comprises a positive electrode. The positive electrode is electrically coupled to the positive terminal. The positive electrode comprises a current collector made of a metal, preferably aluminum. The current collector contacts the positive terminal. The positive electrode comprises a positive electrode material.

[0091] Fabrication of Negative Electrode - Example 1

[0092] A carboxymethyl cellulose (CMC) binder is provided and optionally mixed with water. The proportion of the CMC binder is 2 wt%.

[0093] Carbon black (CB) was added as a first conductive additive in a ratio of 5 wt %.

[0094] Adding activated carbon (AC) particles and Nb 2 O 5 Particles are used as negative electrode active materials. Nb 2 O 5 The particles are composed of orthorhombic Nb 2 O 5 In addition to the inevitable impurities, the negative electrode active material constitutes the remainder of 100wt%. The negative electrode active material is composed of 60wt% Nb 2 O 5 particles and 40wt% AC particles.

[0095] The particle size D90 of AC particles is 10μm to 15μm, Nb 2 O 5 The particles have a particle size D90 of 0.5 μm to 60 μm. The AC particles may be carbide derived carbon (e.g. from SiC or TiC) and have a particle size greater than 1000 μm. 2 / g of BET nitrogen surface area.

[0096] Styrene butadiene rubber (SBR) was added as a second binder in a ratio of 2 wt%.

[0097] After mixing, a slurry is obtained that can be distributed on a conductive electrode substrate (eg, current collector).

[0098] The coated substrate is then heated to remove possible solvents and cure the binder, thereby forming a negative electrode.

[0099] Example 2

[0100] The method of Example 1 was repeated (except that the proportions of some components of the composition were different). The binder remained unchanged. CB was added at a proportion of 4 wt%. Carbon nanotubes (CNT) as a second conductive additive were added together with carbon black at a proportion of 0.5 wt%. The proportions of the negative electrode active materials were adjusted accordingly.

[0101] Example 3

[0102] The method of Example 2 was repeated (except that the proportions of some components of the composition were different). The binder remained unchanged. Carbon black (CB) was added at a proportion of 2 wt%. CNT was added at a proportion of 0.5 wt%. The proportions of the negative electrode active materials were adjusted accordingly.

[0103] The following Table 1 summarizes the available gravimetric capacities of the negative electrodes according to Examples 1 to 3.

[0104] Table 1

[0105]

[0106] Example 4

[0107] The method of Example 1 to Example 3 is repeated, wherein Nb 2 O 5 The content of the particles was changed to 30 wt%, 40 wt%, 50 wt% and 70 wt%. The content of the AC particles was adjusted to 70 wt%, 60 wt%, 50 wt% and 30 wt% accordingly.

[0108] Example 5

[0109] The methods of Examples 1 to 3 were repeated, wherein the particle size D90 of the AC particles was changed to 20 μm to 50 μm.

[0110] Fabrication of Positive Electrode - Example 1

[0111] A carboxymethyl cellulose (CMC) binder is provided and optionally mixed with water. The proportion of the CMC binder is 4 wt%.

[0112] Carbon black (CB) was added at a ratio of 2 wt % and carbon nanotubes (CNT) were added at a ratio of 1 wt %.

[0113] Adding Nb-LiMn 2 O 4 The (Nb-LMO) particles serve as the positive electrode active material and constitute the main body of the positive electrode material.

[0114] The acrylic adhesive was added as the second adhesive at a ratio of 2 wt %.

[0115] After mixing, a slurry is obtained that can be distributed on a conductive electrode substrate (eg, current collector).

[0116] The coated substrate is then heated in order to remove possible solvents and cure the binder, thereby forming the positive electrode.

[0117] Example 2

[0118] The method of Example 1 was repeated (except that the proportions of some components of the composition were different). The proportion of CMC binder was 2wt%, and the proportion of acrylic binder was 2wt%. Carbon black (CB) was added at a proportion of 2wt%. Carbon nanotubes (CNT) were added at a proportion of 1wt%. The electrolyte consisted of 90vol% acetonitrile and 10vol% ethylene carbonate and 1M LiPF 6 The following Table 2 shows the corresponding electrochemical performance.

[0119] Example 3

[0120] The method of Example 1 was repeated (except that the proportions of some components of the composition were different). The proportion of CMC binder was 2wt%, and the proportion of acrylic binder was 2wt%. 2wt% of CB was used, and 0.5wt% of CNT and 0.5wt% of graphene were used. The electrolyte consisted of 50vol% acetonitrile and 50vol% ethylene carbonate and 1M LiPF 6 The following Table 2 shows the corresponding electrochemical performance.

[0121] Table 2

[0122]

[0123] Composition of the electrolyte - Example 1

[0124] By mixing 90 vol% acrylonitrile (ACE) and 10 vol% ethylene carbonate (EC), and adding a certain amount of LiPF 6 , so that the ist concentration in the liquid component is 1 mol / L, thereby obtaining an organic anhydrous electrolyte.

[0125] Example 2

[0126] Organic anhydrous electrolytes were obtained by changing the content of ACE to 85 vol%, 88 vol%, 89 vol%, 91 vol%, 93 vol% and 95 vol% and adjusting the content of EC accordingly. The concentration of LiPF6 remained unchanged.

[0127] Example 3

[0128] By mixing as described in Example 1 and Example 2, an organic anhydrous electrolyte is obtained, wherein LiPF 6 The concentration changed to 0.5mol / L, 1.5mol / L, 2mol / L and 3mol / L.

[0129] Example 4

[0130] By performing the mixing as described in Example 1 to Example 2, an organic anhydrous electrolyte is obtained, wherein LiPF 6Replaced by one of the following conductive salts: lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4 ), lithium hexafluorophosphate (LiPF 6 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium trifluoromethanesulfonate (LiSO 3 CF 3 ), lithium bis(trifluoromethylsulfonyl)imide (LiN(SO 2 CF 3 ) 2 ), lithium bis(pentafluoroethanesulfonyl)imide (LiN(SO 2 C 2 F 5 ) 2 ), lithium bis(oxalate)borate (LiBOB, LiB(C 2 O 4 ) 2 ), lithium difluoro(oxalato)borate (LiBF 2 (C 2 O 4 )), lithium tris(pentafluoroethyl) trifluorophosphate (LiPF 3 (C 2 F 5 ) 3 ) or a mixture thereof.

[0131] In summary, the present invention finds that the aforementioned measures allow the charging rate to be increased by up to 30% compared to conventional batteries with the same nominal capacity. The present invention achieves significant improvements in energy storage batteries (eg, hybrid supercapacitors) and achieves lower ESR and increased energy density.

Claims

1. An energy storage battery for storing electrical energy, the battery comprising a negative electrode and a positive electrode, the negative electrode and the positive electrode being immersed in an organic non-aqueous electrolyte; in, The negative electrode includes a negative active material composition having Nb2O5 particles and activated carbon (AC) particles; The positive electrode comprises a positive electrode active material composition, the positive electrode active material composition mainly comprises a lithium manganese oxide material, the lithium manganese oxide material mainly comprises lithium manganese oxide and 0.001 wt % to 5.0 wt % of niobium based on the weight of the lithium manganese oxide.

2. The energy storage battery according to claim 1, wherein: The negative electrode active material composition includes a negative electrode active material consisting of Nb2O5 particles and AC particles.

3. An energy storage battery according to any one of the preceding claims, wherein: The negative electrode composition and / or the positive electrode composition includes at least one conductive additive.

4. The energy storage battery according to claim 3, wherein: The at least one conductive additive is selected from the group consisting of carbon black (CB), carbon nanotubes (CNT), graphene, and mixtures thereof.

5. An energy storage battery according to any one of the preceding claims, wherein: The negative electrode active material composition consists of greater than 50wt%, preferably greater than 60wt% of negative electrode active material, and / or, wherein the positive electrode active material composition consists of greater than 50wt%, preferably greater than 90wt%, preferably greater than 95wt%, preferably greater than 97wt% or more of positive electrode active material.

6. An energy storage battery according to any one of the preceding claims, wherein: The particle size D90 of the Nb2O5 particles is 1 μm to 100 μm.

7. An energy storage battery according to any one of the preceding claims, wherein: The AC particles have a diameter of at least 60 m 2 / g, preferably at least 1000m 2 / g of BET nitrogen surface area.

8. An energy storage battery according to any one of the preceding claims, wherein: The AC particles have a particle size D90 of 5 μm to 30 μm.

9. The energy storage battery according to any one of claims 4 to 8, wherein: The negative electrode composition and / or the positive electrode composition includes 1 wt % to 10 wt % of carbon black.

10. The energy storage battery according to any one of claims 4 to 9, wherein: The negative electrode composition and / or the positive electrode composition includes 0.3 wt % to 2 wt % of CNTs.

11. The energy storage battery according to any one of claims 4 to 10, wherein: The negative electrode composition and / or the positive electrode composition includes 0.3 wt % to 2 wt % of graphene.

12. The energy storage battery according to claims 10 and 11, wherein: The deviation of the ratio of CNT from the ratio of graphene or the deviation of the ratio of graphene from the ratio of CNT is less than 10%.

13. The energy storage battery according to claim 12, wherein: The ratio of CNT and graphene is the same.

14. An energy storage battery according to any one of the preceding claims, wherein: The electrolyte includes a lithium conductive salt, 80 vol % to 95 vol % of acetonitrile, and 5 vol % to 20 vol % of ethylene carbonate.

15. The energy storage battery according to claim 14, wherein: The lithium conductive salt is selected from the group consisting of lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiSO3CF3), lithium bis(trifluoromethylsulfonyl)imide (LiN(SO2CF3)2), lithium bis(pentafluoroethanesulfonyl)imide (LiN(SO2C2F5)2), lithium bis(oxalate)borate (LiBOB, LiB(C2O4)2), lithium difluoro(oxalate)borate (LiBF2(C2O4)), lithium tris(pentafluoroethyl)trifluorophosphate (LiPF3(C2F5)3) and mixtures thereof.