Epitaxial wafer and preparation method and application thereof
By growing buffer layers and multi-layer roughening layers on the substrate of GaN-based semiconductor materials, using temperature variable growth technology to optimize the growth of roughening layers, solving the problems of low quality of epitaxial layer and high surface roughness, and achieving high quality epitaxiality layer growth and smooth surface.
Patent Information
- Application Number
- CN202310652436.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
During the epitaxial growth process, dislocation and warping are caused by differences in lattice constant and thermal expansion coefficient, resulting in low quality of the epitaxial layer and high surface roughness, making it difficult to obtain a high-quality thin epitaxial layer.
By growing the buffer layer on the substrate and stacking multiple roughened layers on the buffer layer in turn, using temperature variable growth technology, the growth process of the roughened layer is optimized, and the 3D nucleation center is grown to balance longitudinal and lateral growth. A flat surface with a 3D distribution is formed to improve the crystal quality of the epitaxial layer.
The growth of high-quality epitaxial layer is achieved, the surface defects are reduced, the crystal quality and smoothness of the epitaxial layer are improved, and the production cost is reduced.
Smart Images

Figure CN119069340A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors, and in particular relates to an epitaxial wafer and a preparation method and application thereof. Background Art
[0002] GaN-based semiconductor materials have the characteristics of large bandgap, high thermal conductivity, high temperature resistance, radiation resistance, acid and alkali resistance, high strength and high hardness, etc., and are one of the semiconductor materials that people in the world are most interested in. GaN-based semiconductor materials have broad application potential and good market prospects in the fields of high-brightness blue / green / purple / white light diodes, blue / purple lasers, and radiation-resistant, high-temperature and high-power microwave devices.
[0003] However, due to the lack of homogeneous substrates, GaN-based semiconductor materials are usually grown epitaxially using heterogeneous substrates. For example, CN113658853A provides a method for making a GaN heteroepitaxial buffer layer based on Al ion implantation, including the following steps: 1) providing a substrate for GaN heteroepitaxial growth; 2) implanting Al elements into the surface layer of the substrate, wherein the implanted Al element concentration is greater than the Al element solid solubility of the substrate; 3) performing an annealing process on the substrate to repair the lattice defects of the substrate, while allowing the Al elements on the surface layer of the substrate to precipitate from the substrate and form an Al nucleation layer on the surface of the substrate; 4) introducing Al source and N source into the surface of the substrate, and growing an AlN buffer layer on the surface of the substrate based on the Al nucleation layer. Due to the large differences in lattice constants and thermal expansion coefficients between GaN-based semiconductor materials and substrates, a large number of dislocations will be generated during the epitaxial growth process, and the epitaxial film will also warp, and even cracks will appear, which will seriously reduce the film quality of the epitaxial layer. To this end, based on the principle that the out-of-plane tilt angle and in-plane twist angle of the epitaxial layer grains decrease with increasing film thickness, and the crystal quality of the epitaxial layer becomes higher and higher with increasing thickness, it is currently usually necessary to grow a thick nitride epitaxial layer (at least 2μm) to meet the crystal quality requirements.
[0004] Therefore, how to obtain a high-quality thin epitaxial layer at a low cost while reducing the surface roughness of the epitaxial layer is a technical problem that needs to be solved urgently. Summary of the invention
[0005] In view of the deficiencies of the prior art, the purpose of the present invention is to provide an epitaxial wafer and a preparation method and application thereof. The present invention optimizes the growth process of the roughening layer. On the one hand, on the basis of ensuring that the roughening layer grows in the form of a 3D nucleation center, the lateral epitaxial growth process of the epitaxial layer is improved, thereby enhancing the dislocation steering annihilation during the growth process; on the other hand, the distribution of the longitudinal growth and lateral growth of the composite layer is balanced, providing a flat surface with a 3D distribution, ensuring the smooth surface of the epitaxial layer, while reducing the surface defects of the epitaxial layer and improving the crystal quality of the epitaxial layer.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing an epitaxial wafer, the method comprising the following steps:
[0008] (1) growing a buffer layer on a substrate;
[0009] (2) growing a composite layer on the buffer layer, wherein the composite layer comprises at least two roughening layers stacked in sequence, and at least one of the roughening layers is grown in a variable temperature manner;
[0010] (3) Growing an epitaxial layer on the composite layer.
[0011] The present invention optimizes the growth process of the roughened layer. On the one hand, while ensuring that the roughened layer grows in a 3D nucleation center manner, the lateral epitaxial growth process of the epitaxial layer is improved, thereby enhancing the dislocation steering annihilation during the growth process. On the other hand, the distribution of the longitudinal growth and lateral growth of the composite layer is balanced, providing a flat surface with a 3D distribution, ensuring the smooth surface of the epitaxial layer, while reducing the surface defects of the epitaxial layer, improving the crystal quality of the epitaxial layer, and achieving maximum benefits.
[0012] As a preferred technical solution, the composite layer includes a first roughened layer and a second roughened layer stacked in sequence in a direction away from the substrate, and the method for preparing the composite layer includes the following steps:
[0013] (A) heat treating the buffer layer;
[0014] (B) introducing a first precursor with a flow rate of f1 and a second precursor with a flow rate of f2, and growing the first roughening layer on the buffer layer by a variable temperature growth method;
[0015] (C) introducing a third precursor with a flow rate of f3 and a fourth precursor with a flow rate of f4 to grow the second rough layer on the first rough layer.
[0016] By heat treating the buffer layer, the buffer layer can have a 3D nucleation center, which is helpful for the subsequent preparation of a high-quality and thin epitaxial layer.
[0017] As a preferred technical solution, the growth temperature of the buffer layer in step (1) is 500-700°C, for example, 500°C, 550°C, 600°C, 650°C or 700°C.
[0018] As a preferred technical solution, the temperature of the heat treatment in step (A) is 1090-1200°C, for example, it can be 1090°C, 1095°C, 1100°C, 1150°C or 1200°C.
[0019] Preferably, the heat treatment time in step (A) is 10-300 s, for example, it can be 10 s, 50 s, 100 s, 150 s, 200 s, 250 s or 300 s.
[0020] As a preferred technical solution, the variable temperature growth method in step (B) specifically includes the following steps:
[0021] In the process of decreasing the first temperature to the second temperature at the first adjustment rate, a first precursor with a flow rate of f1 and a second precursor with a flow rate of f2 are introduced to grow the first roughened layer on the buffer layer.
[0022] The present invention can rapidly form 3D nucleation centers in the buffer layer by adopting a relatively high temperature heat treatment method; then, by utilizing the temperature change from high to low during the temperature variation process, the 3D nucleation centers formed during the heat treatment process will grow in a growth mode in which the lateral growth ratio is greater than the longitudinal growth ratio during the growth of the first coarsening layer; during the temperature variation process, the lateral growth ratio is gradually replaced by the longitudinal growth ratio; finally, adjacent 3D nucleation center regions are connected through the first coarsening layer and a coarsening layer distribution can be formed in the region between adjacent 3D nucleation centers, providing a growth center with a flat surface and a uniform coarsening layer distribution for the subsequent second coarsening layer, which is beneficial to the rapid merging of the epitaxial layer to achieve a smooth epitaxial layer surface.
[0023] Preferably, the first temperature is the temperature of the heat treatment in step (A).
[0024] Preferably, the second temperature is 1000-1100°C, for example, it may be 1000°C, 1020°C, 1040°C, 1060°C, 1080°C or 1100°C.
[0025] The present invention can achieve longitudinal distribution of the second coarsening layer around the 2D nucleation center at the second temperature, thereby improving the lateral growth of the epitaxial layer and facilitating the acquisition of a high-quality epitaxial layer.
[0026] Preferably, the first adjustment rate is 0-1°C / s and is not 0, for example, it can be 0.2°C / s, 0.4°C / s, 0.6°C / s, 0.8°C / s or 1°C / s.
[0027] In the present invention, if the first adjustment rate is too large, it is difficult to form a uniformly distributed first roughened layer on the substrate surface due to the difference in potential energy on the substrate surface, which ultimately increases the surface roughness of the epitaxial layer and reduces the crystal quality.
[0028] Preferably, the f1 is 10-1000 sccm, for example, it may be 10 sccm, 50 sccm, 100 sccm, 200 sccm, 400 sccm, 600 sccm, 800 sccm or 1000 sccm, etc.
[0029] Preferably, f2 is 2-100slm, for example, 2slm, 5slm, 10slm, 20slm, 40slm, 60slm, 80slm or 100slm, etc.
[0030] As a preferred technical solution, the composite layer further includes a third roughened layer disposed on a side of the second roughened layer away from the first roughened layer, and the method for preparing the composite layer further includes the following steps:
[0031] A fifth precursor with a flow rate of f5 and a sixth precursor with a flow rate of f6 are introduced, and the third roughening layer is grown on the second roughening layer by adopting a variable temperature growth method.
[0032] As a preferred technical solution, the specific steps of growing the third roughening layer include:
[0033] In the process of increasing the second temperature to the third temperature at the second adjustment rate, a fifth precursor with a flow rate of f5 and a sixth precursor with a flow rate of f6 are introduced to grow the third rough layer on the second rough layer.
[0034] The present invention adopts a variable temperature growth method to grow a third roughened layer on the second roughened layer. During the variable temperature growth process from low temperature to high temperature, the third roughened layer can gradually transition from longitudinal growth to lateral growth, which is beneficial to the rapid merging of the epitaxial layers to achieve a smooth epitaxial layer surface. The reflection curve of the grown composite layer presents a V-shape, which indicates that the method provided by the present invention can balance the influence of the 3D roughened layer process on the lateral epitaxial growth process and reduce the surface defects of the epitaxial layer, so as to obtain a smooth, high-quality epitaxial layer.
[0035] As a preferred technical solution, the third temperature is 1100-1200°C, for example, it can be 1100°C, 1120°C, 1140°C, 1160°C, 1180°C or 1200°C.
[0036] Preferably, the second adjustment rate is 0-1°C / s and is not 0, for example, it can be 0.2°C / s, 0.4°C / s, 0.6°C / s, 0.8°C / s or 1°C / s.
[0037] In the present invention, if the second adjustment rate is too large, it is difficult to form a uniformly distributed second roughened layer on the substrate surface due to the difference in potential energy on the substrate surface, which ultimately increases the surface roughness of the epitaxial layer and reduces the crystal quality.
[0038] Preferably, the f5 is 10-1000sccm, for example, it may be 10sccm, 50sccm, 100sccm, 200sccm, 400sccm, 600sccm, 800sccm or 1000sccm, etc.
[0039] Preferably, the f6 is 2-100slm, for example, 2slm, 5slm, 10slm, 20slm, 40slm, 60slm, 80slm or 100slm, etc.
[0040] As a preferred technical solution, the first precursor, the third precursor and the fifth precursor are independently group III A precursors.
[0041] It should be noted that, in the present invention, "independently" means that the first precursor, the third precursor and the fifth precursor can be group III A precursors respectively, and the three can be the same substance or different substances, and the selection of the three does not interfere with each other. The following "independently" is the same.
[0042] Preferably, the Group III A element in the Group III A precursor includes any one of indium (In), gallium (Ga) or aluminum (Al), or a combination of at least two of them.
[0043] Preferably, the Group III A precursor comprises a Group III A organic compound, and the Group III A organic compound comprises any one of an indium source, a gallium source or an aluminum source, or a combination of at least two thereof.
[0044] The present invention does not limit the specific type of the indium source. For example, it can be any one of trimethyl indium, triethyl indium or dimethyl ethyl indium, or a combination of at least two of them.
[0045] The present invention does not limit the specific type of the gallium source. For example, it can be any one of trimethyl gallium, triethyl gallium or triisopropyl gallium, or a combination of at least two of them.
[0046] The present invention does not limit the specific type of the aluminum source. For example, it can be any one of trimethylaluminum, triethylaluminum, dimethylaluminum alkoxide, dimethylaluminum hydride or an alkanes complex, or a combination of at least two thereof.
[0047] Preferably, the second precursor, the fourth precursor and the sixth precursor are independently group VA N source precursors.
[0048] Preferably, the Group VA N source precursor comprises NH3 and / or an organic nitrogen source.
[0049] The present invention does not limit the specific type of the organic nitrogen source. For example, it can be any one of tert-butylamine, n-propylamine or dimethyl hydrazine, or a combination of at least two of them.
[0050] As a preferred technical solution, the preparation method comprises the following steps:
[0051] (1) growing the buffer layer on the substrate at a temperature of 500-700° C.;
[0052] (2) sequentially growing a first roughening layer, a second roughening layer and a third roughening layer on the buffer layer, the specific steps comprising:
[0053] (A) heat treating the buffer layer at a temperature of 1090-1200° C. and a pressure of 50-650 torr for 10-300 seconds;
[0054] (B) in the process of reducing the temperature from the first temperature to the second temperature at the first adjustment rate, introducing the first precursor and the second precursor at a pressure of 100-650 torr to obtain the first roughened layer;
[0055] The first temperature is 1090-1200° C., the second temperature is 1000-1100° C., the first adjustment rate is 0-1° C. / s and is not 0, the flow rate of the first precursor is 10-1000 sccm, the flow rate of the second precursor is 2-100 slm, and the thickness of the first roughening layer is 5-500 nm;
[0056] (C) introducing a third precursor and a fourth precursor at the second temperature and a pressure of 100-650 torr to obtain the second roughened layer;
[0057] Wherein, the flow rate of the third precursor is 10-1000 sccm, the flow rate of the fourth precursor is 2-100 slm, and the thickness of the second roughening layer is 5-100 nm;
[0058] (D) during the process of increasing the temperature from the second temperature to the third temperature at a second adjustment rate, introducing a fifth precursor and a sixth precursor at a pressure of 100-650 torr to obtain the third roughened layer;
[0059] The second adjustment rate is 0-1°C / s and is not 0, the third temperature is 1100-1200°C, the flow rate of the fifth precursor is 10-1000sccm, the flow rate of the sixth precursor is 2-100slm, and the thickness of the third roughening layer is 5-500nm;
[0060] (3) Growing an epitaxial layer on the surface of the third roughened layer at a temperature of 1100-1200° C. and a pressure of 100-400 torr.
[0061] In a second aspect, the present invention provides an epitaxial wafer prepared by the preparation method described in the first aspect, wherein the epitaxial wafer comprises a substrate, a buffer layer, a composite layer and an epitaxial layer stacked in sequence;
[0062] The composite layer includes at least two roughened layers stacked in sequence.
[0063] As a preferred technical solution, the composite layer includes a first roughened layer, a second roughened layer and a third roughened layer which are sequentially stacked in a direction away from the substrate;
[0064] Preferably, the thickness ratio of the first roughening layer, the second roughening layer and the third roughening layer is (5-500):(5-100):(5-500). The selection range of the first roughening layer "5-500" can be, for example, 5, 10, 50, 100, 200, 300, 400 or 500, the selection range of the second roughening layer "5-100" can be, for example, 5, 10, 20, 40, 60, 80 or 100, and the selection range of the third roughening layer "5-500" can be, for example, 5, 10, 50, 100, 200, 300, 400 or 500, etc.
[0065] In the present invention, the thinner second roughening layer not only helps the lateral epitaxial growth of the epitaxial layer, but also lays a foundation for the formation of a smooth surface of the epitaxial layer.
[0066] Preferably, the thickness of the composite layer is 50-100 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0067] Preferably, the buffer layer has a thickness of 10-100 nm, for example, 10 nm, 20 nm, 40 nm, 60 nm, 80 nm or 100 nm.
[0068] Preferably, the thickness of the epitaxial layer is 500-1500 nm, for example, 500 nm, 700 nm, 900 nm, 1100 nm, 1300 nm or 1500 nm.
[0069] Preferably, the surface roughness of the epitaxial layer is 0-100 nm, for example, it can be 0, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0070] In a third aspect, the present invention provides an electronic device, comprising the epitaxial wafer as described in the second aspect.
[0071] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0072] Compared with the prior art, the present invention has the following beneficial effects:
[0073] The present invention optimizes the growth process of the roughened layer. On the one hand, while ensuring that the roughened layer grows in a 3D nucleation center manner, the lateral epitaxial growth process of the epitaxial layer is improved, thereby enhancing the dislocation steering annihilation during the growth process; on the other hand, the distribution of the longitudinal growth and lateral growth of the composite layer is balanced, providing a flat surface with a 3D distribution, ensuring the smooth surface of the epitaxial layer, while reducing the surface defects of the epitaxial layer, improving the crystal quality of the epitaxial layer, and achieving maximum benefit. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] Figure 1 The present invention is a schematic flow chart of a method for preparing an epitaxial wafer.
[0075] Figure 2 This is a schematic diagram of the structure of the epitaxial wafer prepared in Example 1 of the present invention.
[0076] Figure 3 This is a surface AFM image of the epitaxial layer provided in Example 1 of the present invention.
[0077] Figure 4 This is a surface AFM image of the epitaxial layer provided in Example 2 of the present invention.
[0078] Figure 5 This is a surface AFM image of the epitaxial layer provided in Example 3 of the present invention.
[0079] Figure 6 XRD diffraction patterns of the epitaxial layers provided in Examples 1-3 of the present invention.
[0080] Figure 7 This is a surface AFM image of the epitaxial layer provided for Comparative Example 1 of the present invention.
[0081] Figure 8This is a comparison chart of the reflection curve of the composite layer provided in Example 1 of the present invention and the reflection curve of the roughened layer provided in Comparative Example 1.
[0082] Among them, 11 is a substrate; 12 is a GaN buffer layer; 13 is a first GaN roughening layer; 14 is a second GaN roughening layer; 15 is a third GaN roughening layer; and 16 is a GaN epitaxial layer. DETAILED DESCRIPTION
[0083] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0084] See also Figure 1 , Figure 1 The present invention provides a process flow diagram of a method for preparing an epitaxial wafer, wherein the method comprises the following steps:
[0085] S1: growing a buffer layer on a substrate.
[0086] The substrate may be a sapphire substrate, a SiC substrate, a Si substrate, a gallium oxide substrate, a zinc oxide substrate or a diamond substrate, etc.; the thickness of the buffer layer is 10-100 nm; the buffer layer is a nitride buffer layer, and the nitride may be GaN, AlGaN, AlN, InGaN, AlInN, InN or AlGaInN, etc.
[0087] S2: growing a composite layer on the buffer layer, wherein the composite layer comprises at least two roughening layers stacked in sequence, and at least one of the roughening layers is grown in a variable temperature manner.
[0088] The thickness of the composite layer is 50-100 nm.
[0089] S3: growing an epitaxial layer on the composite layer.
[0090] The thickness of the epitaxial layer is 500-1500 nm; the epitaxial layer is a nitride epitaxial layer, and the nitride may be GaN, AlGaN, AlN, InGaN, AlInN, InN or AlGaInN, etc.
[0091] It is worth noting that the above steps S1-S3 can be implemented in a metal organic chemical vapor deposition (MOCVD) device.
[0092] The present invention optimizes the growth process of the roughening layer. On the one hand, while ensuring that the roughening layer grows in a 3D nucleation center manner, the lateral epitaxial growth process of the epitaxial layer is improved, thereby enhancing the dislocation steering annihilation during the growth process. On the other hand, the distribution of the longitudinal growth and lateral growth of the roughening layer is balanced, providing a flat surface with a 3D distribution, ensuring a smooth surface of the epitaxial layer, while reducing the surface defects of the epitaxial layer and improving the crystal quality of the epitaxial layer.
[0093] Example 1
[0094] This embodiment provides an epitaxial wafer, the structural schematic diagram of the epitaxial wafer is as follows Figure 2 As shown, the epitaxial wafer includes a substrate 11, a GaN buffer layer 12, a first GaN roughening layer 13, a second GaN roughening layer 14, a third GaN roughening layer 15 and a GaN epitaxial layer 16 which are stacked in sequence.
[0095] This embodiment also provides a method for preparing the epitaxial wafer, which comprises the following steps:
[0096] (1) A buffer layer with a thickness of 30 nm is grown on the substrate 11 at a temperature of 550°C.
[0097] The substrate 11 is a sapphire substrate with a size of 4 inches; the buffer layer is a GaN buffer layer 12 .
[0098] (2) A composite layer is grown on the GaN buffer layer 12 .
[0099] The composite layer includes a first GaN rough layer 13, a second GaN rough layer 14 and a third GaN rough layer 15, and the specific growth steps include:
[0100] (A) The GaN buffer layer 12 is heat treated for 90 seconds at a temperature of 1095° C. and a pressure of 150 torr.
[0101] (B) While the temperature is reduced from 1095° C. to 1065° C. at a first adjustment rate, the first precursor and the second precursor are introduced at a pressure of 150 torr to obtain a first GaN roughened layer 13 with a thickness of 100 nm.
[0102] The first adjustment rate is 0.75° C. / s; the first precursor is trimethyl gallium (TMG) with a flow rate of 200 sccm; the second precursor is NH 3 with a flow rate of 50 slm.
[0103] This embodiment forms a composite layer with Ga surface distribution, consistent phase and uniform distribution by controlling the growth process of the composite layer.
[0104] (C) Under the conditions of a temperature of 1065° C. and a pressure of 200 torr, the third precursor and the fourth precursor are introduced to obtain a second GaN roughened layer 14 with a thickness of 35 nm.
[0105] The third precursor is TMG with a flow rate of 220 sccm; the fourth precursor is NH3 with a flow rate of 35 slm.
[0106] (D) While the temperature is increased from 1065° C. to 1150° C. at a second adjustment rate, the fifth precursor and the sixth precursor are introduced at a pressure of 150 torr to obtain a third GaN roughened layer 15 with a thickness of 80 nm.
[0107] The second adjustment rate is 1°C / s; the fifth precursor is TMG with a flow rate of 200 sccm; the sixth precursor is NH3 with a flow rate of 50 slm.
[0108] (3) A GaN epitaxial layer 16 with a thickness of 1500 nm is grown on the surface of the third GaN roughened layer 15 at a temperature of 1150° C. and a pressure of 150 torr.
[0109] Example 2
[0110] The difference between this embodiment and embodiment 1 is that the growth thickness of the GaN epitaxial layer is 1000 nm.
[0111] The rest of the preparation methods and parameters were the same as those in Example 1.
[0112] Example 3
[0113] The difference between this embodiment and embodiment 1 is that the growth thickness of the GaN epitaxial layer is 500 nm.
[0114] The rest of the preparation methods and parameters were the same as those in Example 1.
[0115] Figure 3 , Figure 4 and Figure 5 The surface atomic force microscope (AFM) images of the epitaxial layers prepared in Examples 1-3 are shown. Figure 3-5 It can be seen that the surfaces of the epitaxial layers prepared in Examples 1-3 are all smooth and have no pit-shaped defect distribution.
[0116] Figure 6The X-ray diffraction (XRD) diagram of the epitaxial layers prepared in Examples 1-3 is shown, wherein the horizontal axis θ is the diffraction angle and the vertical axis is the intensity of the X-ray diffraction. It can be seen from the figure that the (102) plane diffraction peaks of the epitaxial layers prepared in Examples 1-3 overlap and the half-peak widths are basically the same, indicating that the present invention can achieve the preparation of high-quality epitaxial layers with smooth surfaces.
[0117] Example 4
[0118] This embodiment provides an epitaxial wafer, which includes a substrate, a GaN buffer layer, a first GaN roughening layer, a second GaN roughening layer, a third GaN roughening layer and a GaN epitaxial layer stacked in sequence.
[0119] This embodiment also provides a method for preparing the epitaxial wafer, which comprises the following steps:
[0120] (1) A GaN buffer layer with a thickness of 10 nm was grown on a substrate at a temperature of 600°C.
[0121] The substrate is a sapphire substrate with a size of 4 inches; the buffer layer is a GaN buffer layer.
[0122] (2) Growing a composite layer on the GaN buffer layer.
[0123] The composite layer includes a first GaN roughening layer, a second GaN roughening layer and a third GaN roughening layer, and the specific steps include:
[0124] (A) The GaN buffer layer was heat treated at 1150°C and 300 torr for 300 seconds.
[0125] (B) While the temperature is reduced from 1150° C. to 1000° C. at a first adjustment rate, a first precursor and a second precursor are introduced at a pressure of 300 torr to obtain a first GaN roughened layer with a thickness of 250 nm.
[0126] The first adjustment rate is 0.5°C / s; the first precursor is trimethylgallium, and the flow rate is 500sccm; the second precursor is tert-butylamine, and the flow rate is 10slm.
[0127] (C) Under the conditions of a temperature of 1000° C. and a pressure of 100 torr, a third precursor and a fourth precursor are introduced to obtain a second GaN roughened layer with a thickness of 10 nm.
[0128] The third precursor is trimethylgallium with a flow rate of 500 sccm, and the fourth precursor is tert-butylamine with a flow rate of 10 slm.
[0129] (D) While the temperature is increased from 1000° C. to 1200° C. at a second adjustment rate, the fifth precursor and the sixth precursor are introduced at a pressure of 300 torr to obtain a third GaN roughened layer with a thickness of 250 nm.
[0130] The second adjustment rate is 0.5°C / s; the fifth precursor is trimethylgallium, and the flow rate is 500sccm; the sixth precursor is tert-butylamine, and the flow rate is 10slm.
[0131] (3) A GaN epitaxial layer with a thickness of 1500 nm was grown on the surface of the third GaN roughened layer at a temperature of 1100° C. and a pressure of 250 torr.
[0132] Example 5
[0133] This embodiment provides an epitaxial wafer, which includes a substrate, an AlN buffer layer, a first AlN roughening layer, a second AlN roughening layer, a third AlN roughening layer and an AlN epitaxial layer stacked in sequence.
[0134] This embodiment provides a method for preparing an epitaxial wafer, and the preparation method comprises the following steps:
[0135] (1) An AlN buffer layer with a thickness of 100 nm was grown on a sapphire substrate at a temperature of 700°C.
[0136] (2) Growing a composite layer on the AlN buffer layer.
[0137] The composite layer includes a first AlN roughened layer, a second AlN roughened layer and a third AlN roughened layer, and the specific steps include:
[0138] (A) The AlN buffer layer was heat treated at 1200°C and 650 torr for 10 seconds.
[0139] (B) In the process of decreasing the temperature from the first temperature to the second temperature at the first adjustment rate, the first precursor and the second precursor are introduced at a pressure of 650 torr to obtain a first AlN roughened layer with a thickness of 200 nm.
[0140] The first temperature is 1200° C., the second temperature is 1100° C., and the first adjustment rate is 0.3° C. / s; the first precursor is trimethylaluminum, and the flow rate is 800 sccm; the second precursor is NH3, and the flow rate is 100 slm.
[0141] (C) Under the conditions of the second temperature and the pressure of 600 torr, the third precursor and the fourth precursor are introduced to obtain a second AlN roughened layer with a thickness of 10 nm.
[0142] The third precursor is trimethylaluminum with a flow rate of 800 sccm; the fourth precursor is NH3 with a flow rate of 100 slm.
[0143] (D) In the process of increasing the temperature from the second temperature to the third temperature at the second adjustment rate, the fifth precursor and the sixth precursor are introduced at a pressure of 650 torr to obtain a third AlN roughened layer with a thickness of 200 nm.
[0144] The second adjustment rate is 0.3°C / s, the third temperature is 1100°C, the fifth precursor is trimethylaluminum, and the flow rate is 800sccm; the sixth precursor is NH3, and the flow rate is 100slm.
[0145] (3) Under the conditions of a temperature of 1200° C. and a pressure of 400 torr, an AlN epitaxial layer with a thickness of 1500 nm was grown on the surface of the third AlN roughened layer.
[0146] Example 6
[0147] The difference between this embodiment and embodiment 1 is that step (B) is not performed, that is, the second GaN roughening layer is directly grown after the GaN buffer layer is heat-treated.
[0148] The remaining preparation methods and parameters are the same as those in Example 1 and will not be described in detail here.
[0149] Example 7
[0150] The difference between this embodiment and embodiment 1 is that step (D) is not performed, that is, the growth of the third roughening layer is not performed.
[0151] The remaining preparation methods and parameters are the same as those in Example 1 and will not be described in detail here.
[0152] Example 8
[0153] The difference between this embodiment and embodiment 1 is that the first adjustment rate is 1.5° C. / s.
[0154] The remaining preparation methods and parameters are the same as those in Example 1 and will not be described in detail here.
[0155] Example 9
[0156] The difference between this embodiment and embodiment 1 is that the second adjustment rate is 1.5° C. / s.
[0157] The remaining preparation methods and parameters are the same as those in Example 1 and will not be described in detail here.
[0158] Comparative Example 1
[0159] In this comparative example, conventional GaN epitaxial technology is used to grow a GaN epitaxial layer with a thickness of 1 μm, and a GaN epitaxial wafer is prepared. The specific steps are as follows:
[0160] (1) A GaN buffer layer with a thickness of 30 nm was grown on a sapphire substrate at a temperature of 550°C.
[0161] (2) A 500 nm thick GaN roughening layer was grown on the GaN buffer layer at a temperature of 1055°C.
[0162] (3) A 1 μm thick GaN epitaxial layer was grown on the GaN roughened layer at a temperature of 1105°C.
[0163] Figure 7 The surface AFM image of the epitaxial layer provided in this comparative example is shown. It can be seen from the image that the surface of the GaN epitaxial layer has densely distributed pit-shaped defects.
[0164] Figure 8 A comparison diagram of the reflection curve of the composite layer provided in Example 1 and the reflection curve of the roughening layer provided in Comparative Example 1 is shown, wherein the dotted line represents the reflection curve of the roughening layer provided in Comparative Example 1, and the solid line represents the reflection curve of the composite layer provided in Example 1. For the solution provided in Comparative Example 1, since the roughening layer is mainly grown in 3D longitudinal direction, the roughening layer is in the growth stage (i.e. Figure 8 The reflection curve of the GaN epitaxial layer (in the dashed box) shows a U-shaped distribution. The GaN epitaxial wafer corresponding to this U-shaped distribution curve has a better lateral epitaxy effect and can obtain a high-quality GaN epitaxial layer. However, conventional GaN epitaxial wafers need to grow a GaN epitaxial layer of more than 2μm to make the surface smooth, otherwise the surface of the GaN epitaxial layer will show a pit-shaped defect distribution, and as the thickness of the GaN epitaxial layer decreases, the more defects are distributed, which seriously affects its application in semiconductor devices. The reflection curve of the composite layer provided in Example 1 in the growth section shows a V-shape. On the one hand, on the basis of ensuring that the composite layer grows in a 3D nucleation center manner, the lateral epitaxial growth of the epitaxial layer is improved, thereby enhancing the dislocation steering annihilation during the growth process; on the other hand, the distribution of the longitudinal growth and lateral growth of the composite layer is balanced, providing a flat surface with a 3D distribution, ensuring the smooth surface of the epitaxial layer, while reducing the surface defects of the epitaxial layer and improving the crystal quality of the epitaxial layer.
[0165] Comparative Example 2
[0166] The difference between this comparative example and Example 1 is that both step (B) and step (D) are constant temperature processes, 1080° C. and 1100° C. respectively, rather than variable temperature processes.
[0167] The remaining preparation methods and parameters are the same as those in Example 1 and will not be described in detail here.
[0168] Comparative Example 3
[0169] The difference between this comparative example and Example 1 is that the composite layer is only a roughened layer, that is, step (C) and step (D) are not performed.
[0170] The remaining preparation methods and parameters are the same as those in Example 1 and will not be described in detail here.
[0171] Performance Testing
[0172] The epitaxial wafers prepared in Examples 1-9 and Comparative Examples 1-3 were subjected to an AFM surface roughness Ra test, and an XRD test was performed on the epitaxial wafers. The test results are shown in Table 1.
[0173] Table 1
[0174]
[0175]
[0176] By comparing the data results of Example 1 with those of Examples 6-7, it can be seen that if step (B) or step (D) is omitted, the surface of the obtained epitaxial layer will show more pit-like and eyebrow defects, which seriously affect the surface smoothness of the epitaxial layer and reduce the crystal quality of the epitaxial layer.
[0177] By comparing the data results of Example 1 with Examples 8-9, it can be seen that if the temperature change rate is too fast, it is difficult to form a uniformly distributed second coarsened layer on the substrate surface due to the difference in potential energy on the substrate surface, thereby increasing the surface roughness of the epitaxial layer and reducing the crystal quality.
[0178] By comparing the data results of Example 1 with those of Comparative Example 1, it can be seen that if the conventional GaN epitaxial technology is used to grow the GaN epitaxial layer, the surface of the epitaxial layer has densely distributed pit-shaped defects and the epitaxial layer has high roughness, which seriously affects its application in semiconductor devices.
[0179] By comparing the data results of Example 1 and Comparative Example 2, it can be seen that if the buffer layer is not grown by variable temperature growth, the transition of the lateral growth and longitudinal growth modes during the growth of the roughening layer cannot be regulated, which is not conducive to the nitride epitaxial layer merging process, thereby increasing the surface roughness of the epitaxial layer and reducing the crystal quality of the epitaxial layer.
[0180] By comparing the data results of Example 1 with those of Comparative Example 3, it can be seen that if only the first roughening layer is grown, the longitudinal depth of the roughening layer will be reduced, and the roughening effect of the roughening layer cannot be fully exerted, which will lead to accelerated merging of the epitaxial layer, and dislocations will not have time to turn, thereby reducing the crystal quality of the epitaxial layer.
[0181] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing an epitaxial wafer, characterized in that: The preparation method comprises the following steps: (1) growing a buffer layer on a substrate; (2) growing a composite layer on the buffer layer, wherein the composite layer comprises at least two roughening layers stacked in sequence, and at least one of the roughening layers is grown at a variable temperature; (3) Growing an epitaxial layer on the composite layer.
2. The preparation method according to claim 1, characterized in that: The composite layer comprises a first roughened layer and a second roughened layer which are sequentially stacked in a direction away from the substrate, and the preparation method of the composite layer comprises the following steps: (A) heat treating the buffer layer; (B) introducing a first precursor with a flow rate of f1 and a second precursor with a flow rate of f2, and growing the first roughening layer on the buffer layer by a variable temperature growth method; (C) introducing a third precursor with a flow rate of f3 and a fourth precursor with a flow rate of f4 to grow the second rough layer on the first rough layer.
3. The preparation method according to claim 2, characterized in that: The variable temperature growth method in step (B) specifically includes the following steps: In the process of reducing the first temperature to the second temperature at the first adjustment rate, introducing a first precursor with a flow rate of f1 and a second precursor with a flow rate of f2 to grow the first roughening layer on the buffer layer; Preferably, the first temperature is the temperature of the heat treatment in step (A).
4. The preparation method according to claim 2, characterized in that: The composite layer further includes a third roughened layer disposed on a side of the second roughened layer away from the first roughened layer, and the method for preparing the composite layer further includes the following steps: A fifth precursor with a flow rate of f5 and a sixth precursor with a flow rate of f6 are introduced, and the third roughening layer is grown on the second roughening layer by adopting a variable temperature growth method.
5. The preparation method according to claim 4, characterized in that: The specific steps of growing the third roughening layer include: In the process of increasing the second temperature to the third temperature at the second adjustment rate, a fifth precursor with a flow rate of f5 and a sixth precursor with a flow rate of f6 are introduced to grow the third rough layer on the second rough layer.
6. The preparation method according to any one of claims 2 to 5, characterized in that: The first precursor, the third precursor and the fifth precursor are independently group IIIA precursors; Preferably, the second precursor, the fourth precursor and the sixth precursor are independently group VA N source precursors.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) growing the buffer layer on the substrate at a temperature of 500-700° C.; (2) sequentially growing a first roughening layer, a second roughening layer and a third roughening layer on the buffer layer, the specific steps comprising: (A) heat treating the buffer layer at a temperature of 1090-1200° C. and a pressure of 50-650 torr for 10-300 seconds; (B) in the process of reducing the temperature from the first temperature to the second temperature at the first adjustment rate, introducing the first precursor and the second precursor at a pressure of 100-650 torr to obtain the first roughened layer; The first temperature is 1090-1200° C., the second temperature is 1000-1100° C., the first adjustment rate is 0-1° C. / s and is not 0, the flow rate of the first precursor is 10-1000 sccm, the flow rate of the second precursor is 2-100 slm, and the thickness of the first roughening layer is 5-500 nm; (C) introducing a third precursor and a fourth precursor at the second temperature and a pressure of 100-650 torr to obtain the second roughened layer; Wherein, the flow rate of the third precursor is 10-1000 sccm, the flow rate of the fourth precursor is 2-100 slm, and the thickness of the second roughening layer is 5-100 nm; (D) during the process of increasing the temperature from the second temperature to the third temperature at a second adjustment rate, introducing a fifth precursor and a sixth precursor at a pressure of 100-650 torr to obtain the third roughened layer; The second adjustment rate is 0-1°C / s and is not 0, the third temperature is 1100-1200°C, the flow rate of the fifth precursor is 10-1000sccm, the flow rate of the sixth precursor is 2-100slm, and the thickness of the third roughening layer is 5-500nm; (3) Growing an epitaxial layer on the surface of the third roughened layer at a temperature of 1100-1200° C. and a pressure of 100-400 torr.
8. An epitaxial wafer prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The epitaxial wafer comprises a substrate, a buffer layer, a composite layer and an epitaxial layer which are stacked in sequence; The composite layer includes at least two roughened layers stacked in sequence.
9. The epitaxial wafer according to claim 8, characterized in that: The composite layer includes a first roughened layer, a second roughened layer and a third roughened layer which are sequentially stacked in a direction away from the substrate; Preferably, the thickness ratio of the first roughened layer, the second roughened layer and the third roughened layer is (5-500):(5-100):(5-500); Preferably, the thickness of the composite layer is 50-100 nm; Preferably, the thickness of the buffer layer is 10-100 nm; Preferably, the thickness of the epitaxial layer is 500-1500 nm; Preferably, the surface roughness of the epitaxial layer is 0-100 nm.
10. An electronic device, characterized in that: The electronic device comprises the epitaxial wafer according to claim 8 or 9.
Citation Information
Patent Citations
Manufacturing method of GaN heteroepitaxial buffer layer based on Al ion implantation
CN113658853A