SiC junction barrier Schottky diode and preparation method thereof
By designing multiple well regions and dielectric layers in SiC junction barrier Schottky diodes, the leakage current problem of SiC junction barrier Schottky diodes under high temperature reverse bias voltage is solved, and the device's surge resistance is improved and performance.
Patent Information
- Application Number
- CN202411197742.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The existing SiC junction barrier Schottky diodes have a large leakage current at high temperature reverse bias voltage and have poor surge resistance.
A SiC junction barrier Schottky diode is designed. By forming a plurality of first well regions on the SiC substrate, the width of the well region gradually decreases with depth and is set to a circular vertical projection to increase Schottky contact. Area and formation of multiple PN junctions reduce the electric field strength of the Schottky region surface, reduce leakage current, and improve the device's surge resistance through the dielectric layer and passivation layer.
It effectively reduces the forward conduction voltage drop, reduces leakage current during reverse bias, improves the device's surge resistance and improves overall performance.
Smart Images

Figure CN119069542A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a SiC junction barrier Schottky diode and a preparation method thereof. Background Art
[0002] In the field of power devices, compared with traditional material Si, SiC material has a faster bandgap width, and the device has better voltage and high temperature resistance. Silicon carbide devices have excellent breakdown resistance, so under the same electrical performance requirements, silicon carbide devices can have a thinner thickness than silicon-based devices. At the same time, silicon carbide devices have a smaller on-resistance, which can reduce forward conduction losses and improve conversion efficiency.
[0003] SiC power diodes are an important branch of SiC power devices, mainly including Schottky barrier diodes (SBD), PIN (Positive intrinsic negative) diodes and junction barrier Schottky diodes (JBS). SBD is a unipolar device with a low turn-on voltage and conduction voltage drop; but in reverse, due to the Schottky barrier, its reverse current is also large. The PIN diode has a small reverse leakage current, but its turn-on voltage is high, so the switching loss is large. The silicon carbide junction barrier Schottky combines the advantages of the two devices, adding a P+ doped region to the Schottky contact of the SBD. When the device is reversed, the depletion region generated by the P+ region and the N-type epitaxial depletion shields the high electric field on the Schottky contact and reduces the leakage current. Therefore, the JBS has both the excellent switching characteristics of the SBD and the high blocking capability close to the PIN diode. At present, there is still room for reducing the forward conduction voltage drop of JBS, and ordinary JBS will increase the leakage current under high temperature reverse bias voltage due to the tunnel effect and defects between the SiC contact area of the Schottky metal layer, and has poor surge resistance. Summary of the invention
[0004] In view of the problems in the prior art, the object of the present invention is to provide a SiC junction barrier Schottky diode, which reduces the on-state voltage of the diode to reduce the leakage current and improve the performance of the diode.
[0005] An embodiment of the present invention provides a SiC junction barrier Schottky diode, comprising:
[0006] A SiC substrate of a first conductivity type including a first surface and a second surface opposite to each other;
[0007] A SiC epitaxial layer of a first conductivity type is located on the first surface of the SiC substrate; wherein the doping concentration of the SiC epitaxial layer is less than the doping concentration of the SiC substrate;
[0008] A well region of the second conductivity type extends from a side of the SiC epitaxial layer away from the SiC substrate into the SiC epitaxial layer; the well region includes a plurality of first well regions and a second well region, the width of the first well region gradually decreases with the depth of the first well region extending into the SiC epitaxial layer, and the vertical projection of the first well region on the SiC substrate is a circle; the SiC epitaxial layer includes a junction barrier region and a terminal region, the terminal region extends from the terminal end of the junction barrier region away from both sides of the junction barrier region; the first well region is located in the junction barrier region, and the second well region is located in the terminal region;
[0009] a dielectric layer, located on a side of the SiC epitaxial layer away from the SiC substrate and covering the terminal region;
[0010] A first electrode layer, located on a side of the SiC epitaxial layer away from the SiC substrate and covering the junction barrier region;
[0011] A second electrode layer is located on the second surface of the SiC substrate.
[0012] In some embodiments, the first well regions are distributed in a regular triangle shape.
[0013] In some embodiments, the dielectric layer is a SiO2 layer.
[0014] In some embodiments, the first conductivity type is N-type, and the second conductivity type is P-type.
[0015] In some embodiments, the first conductivity type is P type, and the second conductivity type is N type.
[0016] The embodiment of the present invention further provides a method for preparing a SiC junction barrier Schottky diode, which is used to prepare the SiC junction barrier Schottky diode as described above, and the method comprises the steps of:
[0017] Providing a SiC substrate of a first conductivity type;
[0018] Forming a SiC epitaxial layer of the first conductivity type on the first surface of the SiC substrate of the first conductivity type; wherein the doping concentration of the SiC epitaxial layer is less than the doping concentration of the SiC substrate;
[0019] A well region of a second conductivity type is formed on the SiC epitaxial layer, wherein the well region extends from a first surface of the SiC epitaxial layer away from the SiC substrate into the SiC epitaxial layer; the well region comprises a plurality of first well regions and a second well region, wherein the width of the first well region gradually decreases with the depth of the first well region extending into the SiC epitaxial layer, and the vertical projection of the first well region on the SiC substrate is a circle; the SiC epitaxial layer comprises a junction barrier region and a terminal region, wherein the terminal region extends from the terminal end of the junction barrier region away from both sides of the junction barrier region; the first well region is located in the junction barrier region, and the second well region is located in the terminal region;
[0020] forming a first electrode layer on a surface of the SiC epitaxial layer away from the SiC substrate, wherein the first electrode layer covers the junction barrier region;
[0021] forming a dielectric layer on a surface of the SiC epitaxial layer away from the SiC substrate, wherein the dielectric layer covers the terminal region;
[0022] A second electrode layer is formed on the second surface of the SiC substrate.
[0023] In some embodiments, the forming of a well region of the second conductivity type on the SiC epitaxial layer comprises the following steps:
[0024] forming a first mask on a side of the SiC epitaxial layer away from the SiC substrate;
[0025] Through exposure, development, etching and a first implantation process, a first sub-well region with a first implantation morphology is formed in the junction barrier region, and a second well region is formed at the termination end;
[0026] forming a second mask on a side of the SiC epitaxial layer away from the SiC substrate;
[0027] Through exposure, development, etching and second injection processes, a second sub-well region is formed in the junction barrier region, and the first sub-well region and the second sub-well region form the first well region; the well depth of the first sub-well region is smaller than the well depth of the second sub-well region, and at the same well depth, the width of the first sub-well region is larger than the width of the first sub-well region.
[0028] In some embodiments, the first mask and the second mask include a SiO 2 layer and a photoresist.
[0029] In some embodiments, the energy of the second implantation process is less than the energy of the first implantation process.
[0030] In some embodiments, the method further comprises the steps of:
[0031] forming a passivation layer on a side of the dielectric layer away from the SiC substrate, wherein the passivation layer covers the dielectric layer;
[0032] A PI layer is formed on a side of the passivation layer away from the SiC substrate, and the PI layer covers the passivation layer.
[0033] In some embodiments, the passivation layer includes a SiN layer.
[0034] The SiC junction barrier Schottky diode and the preparation method thereof provided by the present invention have the following advantages:
[0035] By setting the first well region to be a circle as a vertical projection on the SiC substrate, the contact area between the first electrode layer and the first well region is reduced, that is, the Schottky contact area is increased, so that when forward conduction occurs, the front conduction voltage drop can be reduced; multiple first well regions form multiple PN junctions with the epitaxial layer, and the first well region is set to have a width that gradually decreases with the depth of the first well region extending into the SiC epitaxial layer, which can effectively reduce the electric field strength on the surface of the Schottky region, reduce the leakage current during reverse bias, and at the same time share the surge current, thereby providing the device with surge resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Other features, objectives and advantages of the present invention will become more apparent from a reading of the detailed description of non-limiting embodiments made with reference to the following accompanying drawings.
[0037] Figure 1 is a schematic structural diagram of a SiC junction barrier Schottky diode provided by an embodiment of the present invention;
[0038] Figure 2 is a schematic diagram of a first well region of a SiC junction barrier Schottky diode being set to be circular;
[0039] Figure 3 is a schematic diagram of a first well region of a SiC junction barrier Schottky diode being set in a strip shape;
[0040] Figure 4 It is a flow chart of a method for preparing a SiC junction barrier Schottky diode provided by one embodiment of the present invention;
[0041] Figures 5 to 9 It is a cross-sectional view of the process flow of a method for preparing a SiC junction barrier Schottky diode provided in one embodiment of the present invention.
[0042] Reference numerals:
[0043] 10 SiC substrate
[0044] 20 SiC epitaxial layer
[0045] 30 Well region
[0046] 31 First well region
[0047] 311 First Sub-well Region
[0048] 312 Second sub-well region
[0049] 313 The third sub-well region
[0050] 32 Second well region
[0051] 40 Dielectric layer
[0052] 50 first electrode layer
[0053] 60 Second electrode layer
[0054] 70 Passivation layer
[0055] 80 PI layer DETAILED DESCRIPTION
[0056] The example embodiments will now be described more fully with reference to the accompanying drawings. However, the example embodiments can be implemented in a variety of forms and should not be construed as being limited to the embodiments set forth herein; on the contrary, these embodiments are provided so that the present invention will be comprehensive and complete, and the concept of the example embodiments will be fully conveyed to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their repeated descriptions will be omitted. In the representations of the present application, the reference terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics represented in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. Moreover, the specific features, structures, materials or characteristics represented can be combined in any one or more embodiments or examples in a suitable manner. In addition, the different embodiments or examples represented in the present application and the features of the different embodiments or examples can be combined and combined by those skilled in the art without contradicting each other.
[0057] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the representation of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0058] It should be further understood that the terms "comprises" and "includes" indicate the presence of features, steps, operations, elements, components, items, kinds, and / or groups, but do not exclude the presence, occurrence, or addition of one or more other features, steps, operations, elements, components, items, kinds, and / or groups. The terms "or" and "and / or" used herein are interpreted as inclusive, or mean any one or any combination. Therefore, "A, B or C" or "A, B and / or C" means "any of the following: A; B; C; A and B; A and C; B and C; A, B and C". Exceptions to this definition will only occur when the combination of elements, functions, steps or operations is inherently mutually exclusive in some way.
[0059] To solve the problems in the prior art, an embodiment of the present invention provides a SiC junction barrier Schottky diode. Figure 1 FIG. 2 shows a SiC junction barrier Schottky diode provided by an embodiment of the present invention. Figure 1 As shown, the SiC junction barrier Schottky diode provided by the embodiment of the present invention includes a first conductivity type SiC substrate 10, a first conductivity type silicon carbide epitaxial layer 20, a second conductivity type well region 30, a dielectric layer 40, a first electrode layer 50 and a second electrode layer 60.
[0060] Please continue reading Figure 1 The first conductive type SiC substrate 10 includes a first surface and a second surface opposite to each other. In the embodiment of the present invention, the first surface is the upper surface of the SiC substrate 10, and the second surface is the lower surface of the SiC substrate 10. The first conductive type SiC epitaxial layer 20 is located on the first surface of the SiC substrate 10; wherein the doping concentration of the SiC epitaxial layer 20 is less than the doping concentration of the SiC substrate 10.
[0061] The well region 30 of the second conductivity type extends from one side of the SiC epitaxial layer 20 away from the SiC substrate 10 into the SiC epitaxial layer 20; the well region 30 includes a plurality of first well regions 31 and second well regions 32, the width of the first well region 31 gradually decreases with the depth of the SiC epitaxial layer 20, and the vertical projection of the first well region 31 on the SiC substrate 10 is circular; the SiC epitaxial layer 20 includes a junction barrier region and a terminal region, and the terminal region extends from the terminal end of the junction barrier region away from both sides of the junction barrier region; the first well region 31 is located in the junction barrier region, and the second well region 32 is located in the terminal region. The first well region 31 is conical. In some preferred embodiments, the first well regions 31 are distributed in a regular triangle.
[0062] Here, the width of the first well region 31 gradually decreases with the depth of the first well region 31 extending into the SiC epitaxial layer 20 , that is, the closer the first well region 31 is to the SiC substrate 10 , the smaller the width is, and the farther the first well region 31 is from the SiC substrate 10 , the larger the width is.
[0063] Figure 2 and Figure 3 Schematic diagrams are shown when the first well region 31 is circular and strip-shaped. Figure 2 and Figure 3 In the figure, when the width d of the stripe and the diameter D of the circle are 3 μm, 5 μm, and 7 μm respectively, the Schottky contact area of the first well region 31 of the JBS diode designed as a circle is 21.8%, 27.3%, and 25.6% higher than that of the first well region 31 designed as a stripe. Therefore, the JBS diode with the first well region 31 designed as a circle has a larger Schottky contact area.
[0064] In this embodiment, the first conductivity type is N type, and the second conductivity type is P type. In another embodiment, the first conductivity type may be P type, and the second conductivity type may be N type.
[0065] The dielectric layer 40 is located on the side of the terminal region away from the SiC substrate 10, on the side of the SiC epitaxial layer 20 away from the SiC substrate 10, and covers the terminal region. The dielectric layer here is a SiO2 layer, which is used to eliminate the electric field in the edge region and improve the reverse withstand voltage value of the JBS diode.
[0066] The first electrode layer 50 is located on the side of the SiC epitaxial layer 20 away from the SiC substrate 10 and covers the junction barrier region; the second electrode layer 60 is located on the second surface of the SiC substrate 10. The first electrode layer 50 contacts a portion of the SiC epitaxial layer 20 of the first conductivity type, and the contacted portion forms a Schottky junction J1. The first electrode layer 50 contacts the first well region 31 of the second conductivity type and forms an ohmic contact. A PN junction J2 is formed between the well region 30 of the second conductivity type (including the first well region 31 and the second well region 32) and the SiC epitaxial layer 20 of the first conductivity type.
[0067] In forward operation, the Schottky junction J1 has a lower potential barrier, so when the forward voltage can overcome the barrier height of the Schottky junction J1, the SiC junction barrier Schottky diode can be turned on. Therefore, at a low forward voltage, the JBS diode exhibits Schottky diode characteristics.
[0068] However, in the case of reverse bias, the barrier on one side of the semiconductor increases, and the depletion region formed by the junction J2 between the second conductivity type well region 30 (the first well region 31 and the second well region 32) and the first conductivity type SiC epitaxial layer 20 expands to block the reverse current through the diode, protect the Schottky junction J1 and limit the reverse leakage current in the diode. Therefore, in the case of reverse bias, the SiC junction barrier Schottky diode behaves like a PIN diode.
[0069] By setting the first well region 31 in a circular shape on the SiC substrate, the contact area between the first electrode layer 50 and the first well region 31 is reduced, that is, the Schottky contact area is increased, so that when forward conduction occurs, the front conduction voltage drop can be reduced; multiple first well regions 31 form multiple PN junctions with the epitaxial layer 20, and the first well region 31 is set so that its width gradually decreases with the depth of its extension into the SiC epitaxial layer 20, which can effectively reduce the electric field strength on the surface of the Schottky region, reduce the leakage current during reverse bias, and at the same time share the surge current to provide the device with surge resistance.
[0070] like Figure 4 As shown, the embodiment of the present invention also provides a process flow of a junction barrier Schottky diode. Figures 5 to 9 , describing the process flow of preparing the silicon carbide junction barrier Schottky diode.
[0071] Step S100 : providing a SiC substrate 10 of a first conductivity type.
[0072] Step S200: forming a first conductivity type SiC epitaxial layer 20 on a first conductivity type SiC substrate 10; wherein the doping concentration of the SiC epitaxial layer 20 is less than the doping concentration of the SiC substrate 10, and obtaining Figure 3 The structure shown.
[0073] Specifically, when preparing the SiC epitaxial layer 20 of the first conductivity type, the SiC substrate 10 of the first conductivity type is first pretreated, and then the SiC epitaxial layer 20 of the first conductivity type is grown by a deposition method. The deposition method is, for example, CVD (Chemical Vapor Deposition) and metal organic compound vapor deposition. The first conductivity type may be one of N-type or P-type, and the second conductivity type may be the other of P-type or N-type. In this embodiment, the first conductivity type is P-type, and the second conductivity type is N-type. Therefore, the SiC substrate 10 of the first conductivity type may be an N+ type SiC substrate, and the SiC epitaxial layer 20 of the first conductivity type is an N-type SiC substrate. The doping impurities of the first conductivity type include, but are not limited to, nitrogen (N) or phosphorus (P), etc. Here, the doping impurities of the SiC substrate 10 of the first conductivity type and the SiC epitaxial layer 20 of the first conductivity type may be the same or different, and are not specifically limited here.
[0074] Step S300: forming a well region 30 of a second conductivity type on the SiC epitaxial layer 20, the well region 30 extending from the first surface of the SiC epitaxial layer 20 away from the SiC substrate 10 into the SiC epitaxial layer 20; the well region 30 includes a plurality of first well regions 31 and second well regions 32, the width of the first well region 31 gradually decreases as the depth of the first well region 31 extending into the SiC epitaxial layer 20; the SiC epitaxial layer 20 includes a junction barrier region and a terminal region, the terminal region extending from the terminal end of the junction barrier region away from both sides of the junction barrier region; the first well region 31 is located in the junction barrier region, and the second well region 32 is located in the terminal region. In the embodiment of the present invention, the first well region 31 is conical, and the vertical projection of the first well region 31 on the SiC substrate 10 is circular.
[0075] The second conductivity type well region 30 may be formed by ion implantation of the first conductivity type SiC epitaxial layer 20. In this embodiment, the second conductivity type first well region 31 and the second well region 32 may be represented as a P well. The impurities doped in the formation of the P well include but are not limited to aluminum (Al) and boron (B).
[0076] The formation of the well region 30 of the second conductivity type specifically includes the following steps:
[0077] S310: forming a first mask on a side of the SiC epitaxial layer 20 away from the SiC substrate 10;
[0078] S320: Through exposure, development, etching and the first implantation process, a first sub-well region 311 is formed in the junction barrier region, and a second well region 32 is formed at the termination end. After removing the first mask layer by wet etching, the following is obtained: Figure 6 The structure shown;
[0079] S330: forming a second mask on a side of the SiC epitaxial layer 20 away from the SiC substrate 10;
[0080] S340: through exposure, development, etching and second injection process, a second sub-well region 312 is formed in the junction barrier region, the well depth of the first sub-well region 311 is less than the well depth of the second sub-well region 312, and under the same well depth, the width of the first sub-well region 311 is greater than the width of the second sub-well region 311, and the first mask layer is removed by wet etching to obtain Figure 7 In some embodiments, the first sub-well region 311 and the second sub-well region 312 form the first well region 31. Well depth refers to the diffusion depth of impurity ions.
[0081] It should be noted that the mask includes SiO2 and photoresist. After exposure and development, the photoresist leaves an area to be etched, and after dry etching SiO2, an area on the SiC epitaxial layer 20 for ion implantation is exposed.
[0082] In the embodiment of the present invention, the energy of the second implantation process is less than the energy of the first implantation process. By controlling the implantation energy, the depth of the well region is controlled, so that the width of the well region is reduced as the depth thereof increases.
[0083] The first well region 31 is set to have a width that decreases as it extends into the SiC epitaxial layer 20 by using a multiple injection process. The specific number of injections is set according to the shape of the first well region 31 actually designed, and is not specifically limited here. Figure 1 The first well region 31 of the JBS diode in the Figure 7 The intermediate structure shown in FIG. 1 is implanted again to form a third sub-well region 313, and finally the structure shown in FIG. Figure 8 The structure shown in FIG. 1 , namely, the first sub-well region 311, the second sub-well region 312 and the third sub-well region 313 constitute Figure 1 The third injection process can refer to the process of preparing the first sub-well region 311 and the second sub-well region 312, which will not be described again.
[0084] Step S400: Fig. 9 As shown, a first electrode layer 50 is formed on a side of the SiC epitaxial layer 20 away from the SiC substrate 10 , and the first electrode layer 50 covers the junction barrier region.
[0085] Step S500 : forming a dielectric layer 40 on a surface of the SiC epitaxial layer 20 away from the SiC substrate 10 , wherein the dielectric layer 40 covers the terminal region.
[0086] In this embodiment, the first electrode layer 50 is an anode layer, and the anode layer can be one or more combinations of Ti, Ni, Al, and Cu. The first electrode layer 50 can be a metal layer formed by electron beam evaporation or sputtering.
[0087] Specifically, a dielectric layer 40 made of silicon dioxide is grown on the first conductivity type SiC epitaxial layer 20 by using PECVD technology.
[0088] Step S600: Fig. 9 As shown, a second electrode layer 60 is formed on the second surface of the SiC substrate 10 .
[0089] In this embodiment, the second electrode layer 60 is a cathode layer, and the cathode layer can be one or more combinations of Ti, Ni, Ag, and Pt. Similarly, the second electrode layer 60 can be formed by electron beam evaporation or sputtering process. Rapid thermal annealing is performed in a vacuum environment or an inert gas atmosphere to form an ohmic contact electrode, i.e., a cathode electrode, on the lower surface of the first conductive type silicon carbide.
[0090] Furthermore, the preparation method further comprises the steps of:
[0091] A passivation layer 70 is formed on a side of the dielectric layer 40 away from the SiC substrate 10 , and the passivation layer 70 covers the dielectric layer 40 ;
[0092] A PI layer 80 is formed on the side of the passivation layer 70 away from the SiC substrate 10. The PI layer 80 covers the passivation layer 70. Figure 1 The structure shown.
[0093] The passivation layer 70 includes a SiN layer, which is used to prevent water vapor from damaging the performance of SiO2 and thus affecting the normal performance of the junction barrier Schottky diode. The material of the PI layer is polyimide, which can effectively protect the JBS diode from the influence of the external environment, such as moisture, oxygen and other pollutants, improve the reliability and stability of the JBS diode, and ensure that the JBS device can maintain excellent performance in various environments.
[0094] The SiC junction barrier Schottky diode and the preparation method thereof provided by the present invention have the following advantages:
[0095] By setting the vertical projection of the first well region on the SiC substrate to be circular, the contact area between the first electrode layer and the first well region is reduced, that is, the Schottky contact area is increased, so that when forward conduction occurs, the front conduction voltage drop can be reduced; multiple first well regions form multiple PN junctions with the epitaxial layer, and the first well region is set to have a width that gradually decreases with the depth of the first well region extending into the SiC epitaxial layer, which can effectively reduce the electric field strength on the surface of the Schottky region, reduce the leakage current during reverse bias, and at the same time share the surge current, providing the device with surge resistance.
[0096] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A SiC junction barrier Schottky diode, characterized in that: include: A SiC substrate of a first conductivity type including a first surface and a second surface opposite to each other; A SiC epitaxial layer of a first conductivity type is located on the first surface of the SiC substrate; wherein the doping concentration of the SiC epitaxial layer is less than the doping concentration of the SiC substrate; A well region of the second conductivity type extends from a side of the SiC epitaxial layer away from the SiC substrate into the SiC epitaxial layer; the well region includes a plurality of first well regions and a second well region, the width of the first well region gradually decreases with the depth of the first well region extending into the SiC epitaxial layer, and the vertical projection of the first well region on the SiC substrate is a circle; the SiC epitaxial layer includes a junction barrier region and a terminal region, the terminal region extends from the terminal end of the junction barrier region away from both sides of the junction barrier region; the first well region is located in the junction barrier region, and the second well region is located in the terminal region; a dielectric layer, located on a side of the SiC epitaxial layer away from the SiC substrate and covering the terminal region; A first electrode layer, located on a side of the SiC epitaxial layer away from the SiC substrate and covering the junction barrier region; A second electrode layer is located on the second surface of the SiC substrate.
2. The SiC junction barrier Schottky diode according to claim 1, characterized in that: The first well regions are distributed in an equilateral triangle.
3. The SiC junction barrier Schottky diode according to claim 1, characterized in that: The dielectric layer is a SiO2 layer.
4. The SiC junction barrier Schottky diode according to claim 1, characterized in that: The first conductivity type is N type, and the second conductivity type is P type.
5. The SiC junction barrier Schottky diode according to claim 1, characterized in that: The first conductivity type is P type, and the second conductivity type is N type.
6. A method for preparing a SiC junction barrier Schottky diode, characterized in that: For preparing the SiC junction barrier Schottky diode according to any one of claims 1 to 5, the method comprises the steps of: Providing a SiC substrate of a first conductivity type; Forming a SiC epitaxial layer of the first conductivity type on the first surface of the SiC substrate of the first conductivity type; wherein the doping concentration of the SiC epitaxial layer is less than the doping concentration of the SiC substrate; A well region of a second conductivity type is formed on the SiC epitaxial layer, wherein the well region extends from a first surface of the SiC epitaxial layer away from the SiC substrate into the SiC epitaxial layer; the well region comprises a plurality of first well regions and a second well region, wherein the width of the first well region gradually decreases with the depth of the first well region extending into the SiC epitaxial layer, and the vertical projection of the first well region on the SiC substrate is a circle; the SiC epitaxial layer comprises a junction barrier region and a terminal region, wherein the terminal region extends from the terminal end of the junction barrier region away from both sides of the junction barrier region; the first well region is located in the junction barrier region, and the second well region is located in the terminal region; forming a first electrode layer on a surface of the SiC epitaxial layer away from the SiC substrate, wherein the first electrode layer covers the junction barrier region; forming a dielectric layer on a surface of the SiC epitaxial layer away from the SiC substrate, wherein the dielectric layer covers the terminal region; A second electrode layer is formed on the second surface of the SiC substrate.
7. The method for preparing a SiC junction barrier Schottky diode according to claim 6, characterized in that: The forming of a well region of the second conductivity type on the SiC epitaxial layer comprises the following steps: forming a first mask on a side of the SiC epitaxial layer away from the SiC substrate; Forming a first sub-well region in the junction barrier region and a second well region in the termination end through exposure, development, etching and a first implantation process; forming a second mask on a side of the SiC epitaxial layer away from the SiC substrate; Through exposure, development, etching and second injection processes, a second sub-well region is formed in the junction barrier region, and the first sub-well region and the second sub-well region form the first well region; the well depth of the first sub-well region is smaller than the well depth of the second sub-well region, and at the same well depth, the width of the first sub-well region is larger than the width of the first sub-well region.
8. The method for preparing a SiC junction barrier Schottky diode according to claim 7, characterized in that: The first mask and the second mask include a SiO2 layer and a photoresist.
9. The method for preparing a SiC junction barrier Schottky diode according to claim 7, characterized in that: The energy of the second implantation process is less than the energy of the first implantation process.
10. The method for preparing a SiC junction barrier Schottky diode according to claim 6, characterized in that: The method further comprises the steps of: forming a passivation layer on a side of the dielectric layer away from the SiC substrate, wherein the passivation layer covers the dielectric layer; A PI layer is formed on a side of the passivation layer away from the SiC substrate, and the PI layer covers the passivation layer.
11. The method for preparing a SiC junction barrier Schottky diode according to claim 10, characterized in that: The passivation layer includes a SiN layer.