Indium-free battery piece and preparation method thereof

By using AZO material as the first transport layer of the composite transport layer in the photovoltaic cell, and combining SnOx and other materials with good resistance as the second transport layer, the high price and toxicity of indium materials are solved, and side insulation is achieved and efficient photoelectric conversion reduces production costs and indium toxicity risks.

CN119069552APending Publication Date: 2024-12-03SUZHOU JBAO TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191400.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing photovoltaic cell has high price and toxicity problems of indium materials in the electroplating copper process. At the same time, due to the insufficient resistance of the TCO layer, the winding phenomenon and conduction leakage are caused, which reduces the photoelectric conversion efficiency of the cell. The edge insulation process is discontinuous, which can easily cause damage to the battery cell.

Method used

The composite transport layer, including AZO material with good conductivity and light transmittance, is used as the first transport layer, and is combined with materials such as SnOx with good resistance as the second transport layer to form a hard film layer, and is removed by wet etching process. The side composite transport layer realizes side insulation, reduces raw material costs, and avoids the use of indium materials.

Benefits of technology

Effectively remove the use of indium materials, reduce the production cost of the battery cells, improve the photoelectric conversion efficiency of the battery cells, ensure the side insulation and production consistency of the battery cells, avoid indium toxic operating environment, and improve the battery cells. reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069552A_ABST
    Figure CN119069552A_ABST
Patent Text Reader

Abstract

The invention discloses an indium-free battery piece and a preparation method thereof, the indium-free battery piece comprises a battery piece body and composite transmission layers, and the composite transmission layers are arranged on the front surface and the back surface of the battery piece body; the composite transmission layer comprises a first transmission layer and a second transmission layer, the first transmission layer is arranged close to the cell body, the second transmission layer is arranged on the side, away from the cell body, of the first transmission layer, and the chemical resistance of the second transmission layer is better than that of the first transmission layer. Through the arrangement that the first transmission layer is matched with the second transmission layer, the composite transmission layer makes up the defect that the first transmission layer is poor in chemical resistance, the composite transmission layer has good conductivity and light transmission, an expensive indium material is not used as the material of the composite transmission layer, and the raw material cost of battery manufacturing is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photovoltaic manufacturing, and in particular to an indium-free battery cell and a preparation method thereof. Background Art

[0002] At present, the industry is continuously improving the power generation efficiency of solar modules in two major industrial links. First, in the production of the cell body, the copper electroplating process is introduced, combined with the yellow light patterning process, so that the overall fine grid line width is less than 20um or even finer. In this way, the shading rate and contact resistance can be reduced, so that the overall cell body conversion efficiency is increased by an average of 0.3% to 0.5%.

[0003] After the cell body is prepared, cleaned and texturized, PECVD is used to prepare the base layer of the cell body. That is, a 5-10nm intrinsic amorphous silicon layer is prepared as a passivation layer. At the same time, on the outside of the intrinsic amorphous silicon layer, a boron-doped P-type microcrystalline silicon layer is prepared on the back surface and a phosphorus-doped N-type microcrystalline silicon layer is prepared on the front surface. At this time, the sides of the cell body will also be deposited and coated in sequence. Next, a composite transmission layer is prepared by vacuum deposition processes such as PVD or RPD, including but not limited to a transparent conductive oxide layer (TCO layer) and a bottom conductive layer. However, the TCO layer is currently made of ITO material due to considerations of lateral conductive transmission, transmittance and chemical resistance. Although ITO has many of the above advantages, its fatal disadvantages are the high price and toxicity of indium. Due to the increased demand for display industries and photovoltaic industries in recent years, the average price of indium in June 2024 was 3,150 yuan / Kg, up 50% from 2023. In the foreseeable future, the price of indium is bound to continue to break through along with the silver price as the display, photovoltaic and other industries develop. Therefore, the next step in reducing costs in the photovoltaic industry after removing silver is to remove indium. Among many TCOs, AZO's conductivity and light transmittance are the best comparable to ITO, and AZO is non-toxic. However, AZO's chemical resistance is not as good as ITO. Therefore, when introducing copper electroplating into the production of photovoltaic cell bodies, AZO has always been excluded.

[0004] Fortunately, when we continued to develop composite TCO layers to replace indium materials, we found that we could take advantage of its low chemical resistance and match it with another TCO layer with good chemical resistance, such as SnOx, SiO2, etc. The two can make up for the performance values ​​of conductivity and light transmittance prepared by ITO thin film alone. However, its process characteristics are that when it is prepared by vacuum process, it will not only deposit on the two surfaces of the cell body, but also deposit and cover its side, so that the entire cell body is in a conductive state, which is commonly known as the wrap-around plating phenomenon. This will cause the conduction of the two surfaces of the cell body to form leakage during the subsequent electroplating deposition process, causing the open circuit voltage Voc of the cell body to decrease, and ultimately reduce the photoelectric conversion efficiency of the cell body. In addition, since the wrap-around deposition is non-uniform or continuous on the side of the cell body. If it is not completely removed, there may be a risk that these microstructures attached to the side will fall off during the subsequent process, which may pose a risk to the reliability of the cell body or components. Therefore, everyone in the industry is trying every possible means to prepare the side insulation structure of the battery cell body.

[0005] The current common practice is to coat the bottom conductive layer and ITO layer around the cell body with an insulating film after development and before electroplating. This can prevent electroplating from occurring on the sides during subsequent electroplating. However, the application process is not continuous with the development and electroplating processes. Instead, after exposure, the cell body must be edge-wrapped, dried, and the cell body collected in a single-piece process, and then the cell body must be processed in multiple pieces by automation. Multiple rounds of collecting, placing, and automated operation make it impossible to produce the cell body in a coherent manner, and it is easy to cause cracks or damage to the cell body during transportation.

[0006] Therefore, how to remove indium and insulate the side edges is still an urgent problem to be solved. Summary of the invention

[0007] In order to overcome the above-mentioned shortcomings, one of the purposes of the present invention is to provide an indium-free battery cell, which can remove expensive indium, reduce the raw material cost of the battery, and solve the problem of side plating of the battery cell, so that the side can be insulated.

[0008] In order to achieve the above purpose, the technical solution adopted by the present invention is: an indium-free battery cell, including a battery cell body, and also including:

[0009] A composite transmission layer, the composite transmission layer is arranged on the front and back sides of the battery cell body;

[0010] The composite transmission layer includes a first transmission layer and a second transmission layer, wherein the first transmission layer is arranged close to the battery cell body, and the second transmission layer is arranged on a side of the first transmission layer away from the battery cell body, and the chemical resistance of the second transmission layer is better than that of the first transmission layer.

[0011] The first transmission layer has good conductivity and light transmittance, but poor chemical resistance. By setting a second transmission layer with good chemical resistance on the first transmission layer, in addition to being used for transmission, a hard film layer is also formed. By setting the first transmission layer with the second transmission layer, the composite transmission layer makes up for the defect of the poor chemical resistance of the first transmission layer, and makes the composite transmission layer have good conductivity and light transmittance, and does not use expensive indium materials as the material of the composite transmission layer, reducing the cost of raw materials for battery production.

[0012] Further, the first transmission layer is a single layer or a composite layer of multiple layers, the thickness of the first transmission layer is 5nm to 120nm, and the material of the first transmission layer is selected from any one or more of aluminum-doped zinc oxide (AZO) material, gallium-doped zinc oxide (GZO) material, and aluminum-gallium co-doped zinc oxide (AGZO). Exemplarily, the thickness of the first transmission layer is 5nm, 20nm, 40nm, 60nm, 80nm, 100nm, 120nm, or a range consisting of any two of them.

[0013] AZO materials include ZnO and Al2O3, and the weight ratio of ZnO and Al2O3 is 90:10 to 99:1. The conductivity and light transmittance of AZO are most comparable to ITO, and AZO is non-toxic. However, the chemical resistance of AZO is not as good as that of ITO (ITO materials include In2O3 and SnO2, and the weight ratio of In2O3 and SnO2 is 90:10 to 99:1). Therefore, AZO has always been excluded in the introduction of copper electroplating into the production of photovoltaic cell bodies. The present application reduces the cost of raw materials for producing batteries by combining a first transmission layer with poor chemical resistance with a second transmission layer with good chemical resistance, and replacing ITO materials with low-cost, non-toxic, conductive and light-transmitting AZO materials as the material of the composite transmission layer.

[0014] Further, the second transmission layer is a single layer or a composite layer of multiple layers, the thickness of the second transmission layer is 5nm to 120nm, and the material of the second transmission layer is selected from any one or more of SnOx tin oxide, silicon oxide SiOx, FTO fluorine-doped tin oxide, and boron-doped zinc oxide (BZO). Exemplarily, the thickness of the second transmission layer is 5nm, 20nm, 40nm, 60nm, 80nm, 100nm, 120nm, or a range consisting of any two thereof.

[0015] Further, the composite transport layer further includes a bottom conductive layer disposed on a side of the second transport layer away from the battery cell body. The thickness of the bottom conductive layer is 30 nm to 120 nm, and the material of the bottom conductive layer is selected from any one or more of gold, silver, platinum, copper, palladium, titanium, nickel, tungsten, bismuth, vanadium, gallium, and rhodium. Exemplarily, the thickness of the bottom conductive layer is 30 nm, 40 nm, 60 nm, 80 nm, 100 nm, 120 nm, or a range composed of any two of them.

[0016] Further, the side surface of the composite transport layer is flush with the side surface of the battery cell body. By setting the side surface of the composite transport layer flush with the side surface of the battery cell body, no insulating region is provided on the back surface of the battery cell body, which can increase the power collection area on the back surface of the battery cell body and improve the photoelectric conversion efficiency of the battery cell body.

[0017] Further, a base layer is further included. The base layer includes a front base layer disposed on the front surface of the battery cell body, a back base layer disposed on the back surface of the battery cell body, and side base layers disposed on the side surfaces of the battery cell body. There are two side base layers, which are integrally connected to the front base layer and the side base layer respectively. The distance Te between the two side base layers satisfies the following relationship: 0.1Tt < Te < 0.95Tt, where Tt is the thickness of the battery cell body. By retaining the side base layers, the side surfaces of the battery cell body are in a slightly conductive state.

[0018] Further, the base layer includes an intrinsic passivation layer and a microcrystalline silicon layer. The intrinsic passivation layer is attached to the battery cell body, and the microcrystalline silicon layer is attached to the intrinsic passivation layer. The thickness of the intrinsic passivation layer is 5 nm to 10 nm, and the thickness of the microcrystalline silicon layer is 10 to 30 nm. Exemplarily, the thickness of the intrinsic passivation layer is 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or a range composed of any two of them, and the thickness of the microcrystalline silicon layer is 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, or a range composed of any two of them.

[0019] A method for manufacturing an indium-free battery cell as described above includes the following steps:

[0020] S1. Prepare a composite transport layer on the front and back surfaces of the battery cell body. The composite transport layer includes a first transport layer, a second transport layer, and a bottom conductive layer disposed in sequence.

[0021] S2. Set a mask layer on the front and back surfaces of the battery cell body. The mask layer is disposed on a side of the bottom conductive layer away from the battery cell body, and the mask layer can cover the composite transport layer on the front and back surfaces of the battery cell body.

[0022] S3. Remove the composite transport layer not covered by the mask layer through a wet etching process, that is, remove the composite transport layer on the side of the solar cell.

[0023] S4. Fabricate an indium-free TCO solar cell body insulated on one side through a yellow light pattern transfer process, a copper electroplating process, and a film stripping and copper back etching process.

[0024] Further, in S1, during the deposition of the composite transport layer, deposit the composite transport layer on both the front and back sides of the solar cell body simultaneously. Completely cover one side of the solar cell body to prepare the composite transport layer, and on the other side of the solar cell body, form an insulating region in the area where the carrier tray contacts and supports the solar cell body.

[0025] Further, in S1, during the deposition of the composite transport layer, first prepare the composite transport layer on one side that does not contact the carrier tray; then flip the solar cell body and prepare the composite transport layer on the other side, completely covering the composite transport layer on the front and back sides of the solar cell body.

[0026] Further, in S3, etch the composite transport layer not covered by the mask layer with an acidic solution, and the acidic solution is an organic acid solution, an inorganic acid solution, or a mixed solution of organic acid and inorganic acid.

[0027] Further, in S3, the acidic solution is selected from any one or more of formic acid, hydrochloric acid, sulfuric acid, and nitric acid.

[0028] Further, in S3, the etching temperature is 20°C to 55°C, the operation time is 1 min to 5 min, and the spray pressure is 1.5 Kg / cm 2 ~5 Kg / cm 2 .

[0029] Further, through a wet etching process, remove part or all of the base layer (2) not covered by the mask layer (4). That is, etch the base layer on the side of the solar cell with an acidic solution to completely remove the base layer on the side of the solar cell, and the base layer on the front or back of the solar cell body is flush with the solar cell body. Or partially etch the base layer on the side of the solar cell, and there is a base layer remaining on the side of the solar cell, but the base layer is not conductive. The distance Te between the two base layers on the side of the solar cell satisfies the following condition: 0.1Tt < Te < 0.95Tt, where Tt is the thickness of the solar cell body.

[0030] The beneficial effect of the present invention is that AZO, GZO or AGZO thin film materials with good conductivity but poor chemical resistance are deposited on the substrate of the battery cell body, which is represented by the first transmission layer. Then, thin film layers such as SnO2, FTO and SiO2 with good chemical resistance are covered on the first transmission layer, which is represented by the second transmission layer. In addition to being used for transmission, the second transmission layer also forms a hard mask. At this time, the bottom conductive layer and the first transmission layer can be etched and removed together with an inorganic acid or an acidic acid or a mixed acid solution. At this time, because the first transmission layer with poor chemical resistance under the hard film layer such as SnO2, FTO and SiO2 has been etched and removed, the second transmission layer with good chemical resistance is also peeled and removed, so that the side of the battery is insulated. In this way, the multi-functional indium removal and cost reduction are achieved, the production is easy, the overall continuous production of the battery cell body is matched, the indium poisoning operating environment is removed, and the leakage is isolated to produce the battery cell with a side insulation structure in combination with the copper electroplating process, so as to achieve overall efficiency improvement and cost reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 It is a schematic diagram of the method of depositing a composite transmission layer on both sides of a cell simultaneously according to the present invention;

[0034] Figure 2 It is a schematic diagram of the layer of depositing a composite transmission layer on a single side of a solar cell according to the present invention;

[0035] Figure 3 A schematic diagram of a cell covering mask layer without an insulating region of the present invention;

[0036] Figure 4 It is a schematic diagram of a cell covering mask layer with an insulating area of ​​the present invention;

[0037] Figure 5 This is a schematic diagram of an indium-free battery cell without an insulating region of the present invention;

[0038] Figure 6 It is a schematic diagram of an indium-free battery cell with an insulating region according to the present invention;

[0039] Figure 7It is a schematic diagram of an indium-free battery cell having a substrate layer on the side without an insulating region of the present invention;

[0040] Figure 8 It is a schematic diagram of an indium-free battery cell with a substrate layer on the side of the insulating region of the present invention.

[0041] Among them: 1. Battery cell body; 2. Base layer; 21. Intrinsic passivation layer; 22. Microcrystalline silicon layer; 3. Composite transmission layer; 31. First transmission layer; 32. Second transmission layer; 33. Bottom conductive layer; 4. Mask layer; 5. Insulation area. DETAILED DESCRIPTION

[0042] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0043] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0044] An embodiment of the present invention provides a method for preparing an indium-free battery cell, comprising the following steps:

[0045] S1. See Appendix Figure 1 and attached Figure 2 As shown, a base layer 2 and a composite transmission layer 3 are prepared on the front and back sides of the battery cell body 1 .

[0046] S11 , preparing a base layer 2 on the front and back sides of the battery cell body 1 .

[0047] The base layer 2 is provided with two layers, which are respectively located on the front and back of the cell body 1. The base layer 2 located on the front of the cell body 1 is the front base layer, and the base layer located on the back of the cell body 1 is the back base layer 2. In the process of preparing the base layer 2 by the PECVD process, due to the wrap-around plating phenomenon, a base layer 2 is also formed on the side of the cell body 1, and the base layer 2 located on the side of the cell body 1 is the side base layer. When preparing the front base layer, a side base layer connected to the front base layer is formed, and when preparing the back base layer, a side base layer connected to the back base layer is formed.

[0048] In some embodiments, the base layer 2 includes an intrinsic passivation layer 21 and a microcrystalline silicon layer 22, the intrinsic passivation layer 21 is arranged in contact with the battery cell body 1, and the microcrystalline silicon layer 22 is arranged in contact with the intrinsic passivation layer 21, the thickness of the intrinsic passivation layer 21 is 5nm to 10nm, and the thickness of the microcrystalline silicon layer 22 is 10 to 30nm.

[0049] S12, depositing a composite transmission layer 3 on the base layer 2, wherein the composite transmission layer 3 comprises a first transmission layer 31, a second transmission layer 32 and a bottom conductive layer 33 which are arranged in sequence.

[0050] In some embodiments, the first transmission layer 31 is located on the side of the substrate layer 2 away from the cell body 1, and the material of the first transmission layer 31 is selected from any one or more of aluminum-doped zinc oxide (AZO) material, gallium-doped zinc oxide (GZO) material, and aluminum-gallium co-doped zinc oxide (AGZO). These materials have good conductivity and light transmittance, but poor chemical resistance. Due to poor chemical resistance, there has been no material that can be used as the TCO layer of the cell. Among them, the AZO material includes ZnO and Al2O3, and the weight ratio of ZnO to Al2O3 is 90:10 to 99:1. The conductivity and light transmittance of AZO are most comparable to ITO (ITO materials include In2O3 and SnO2, and the weight ratio of In2O3 to SnO2 is 90:10 to 99:1), and AZO is non-toxic. However, the chemical resistance of AZO is not as good as that of ITO. Therefore, when introducing copper electroplating into the production of photovoltaic cells, AZO has always been excluded. In the present application, by matching the second transmission layer 32 , the low-cost, non-toxic AZO material with good conductivity and light transmittance is used as the material of the composite transmission layer 3 to replace the ITO material, thereby reducing the raw material cost of producing the battery.

[0051] In some embodiments, the first transmission layer 31 is a single-layer structure, or a multi-layer composite structure, with a thickness of 5 nm to 120 nm.

[0052] In some embodiments, the second transmission layer 32 is disposed on a side of the first transmission layer 31 away from the battery cell body 1, and the chemical resistance of the second transmission layer 32 is better than that of the first transmission layer 31. The material of the second transmission layer 32 has good chemical resistance and is selected from SnO x Tin oxide, silicon oxide SiO x , FTO fluorine-doped tin oxide, boron-doped zinc oxide (BZO) or any one or more thereof.

[0053] By setting a second transmission layer 32 with good chemical resistance on the first transmission layer 31, in addition to being used for transmission, a hard film layer is also formed. The first transmission layer 31 and the second transmission layer 32 are set to make up for the defect of poor chemical resistance of the first transmission layer 31, and have good conductivity and light transmittance, and there is no need to use expensive indium material as the material of the composite transmission layer 3, thereby reducing the raw material cost of battery production.

[0054] In some embodiments, the second transmission layer 32 is a single-layer structure, or a multi-layer composite structure, with a thickness of 5 nm to 120 nm.

[0055] In some embodiments, the bottom conductive layer 33 is arranged on the side of the second transmission layer 32 away from the battery cell body 1, the thickness of the bottom conductive layer 33 is 30nm~120nm, and the material of the bottom conductive layer 33 is selected from any one or more of gold, silver, platinum, copper, palladium, titanium, nickel, tungsten, bismuth, vanadium, gallium, and rhodium.

[0056] See attached Figure 1 As shown, in some embodiments, during the process of depositing the composite transmission layer 3, the composite transmission layer 3 is deposited on both sides of the front and back of the battery cell body 1 at the same time. Since the carrier and the back of the battery cell body 1 abut against each other to support the battery cell body 1, after deposition, the front of the battery cell body 1 is completely covered with the composite transmission layer 3 to be prepared, and an insulating area 5 is formed on the back of the battery cell body 1 in the area where the carrier supports and contacts the battery cell body 1.

[0057] See attached Figure 2As shown, in other embodiments, during the deposition process of preparing the composite transmission layer 3, single-sided preparation can be performed, that is, the composite transmission layer 3 on one single side is prepared first, for example, the front side of the cell body 1 is prepared first, and the front side is not in contact with the carrier; then the cell body 1 is turned over, and the composite transmission layer 3 is prepared on the back side of the other cell body 1. Since the composite transmission layer 3 is deposited on the side of the cell body 1 that is not in contact with the carrier in sequence, the front and back sides of the cell body 1 are fully covered with the composite transmission layer 3, so no insulating area is formed on the side of the cell body. Since no insulating area 5 is provided on the back side of the cell body 1, the electricity receiving area on the back side of the cell body 1 can be increased, and the photoelectric conversion efficiency of the cell body 1 can be improved.

[0058] The process of depositing the composite transmission layer 3 includes but is not limited to vacuum thin film deposition such as PECVD, PVD or RPD, and depositing each functional layer once or multiple times to prepare each functional layer (first composite transmission layer 3, second composite transmission layer 3, bottom conductive layer 33). The purpose is to maximize the conversion efficiency of the battery cell body 1.

[0059] S2. See Appendix Figure 3 and attached Figure 4 As shown, a mask layer 4 is provided on the front and back sides of the cell body 1 , and the mask layer 4 is provided on the side of the bottom conductive layer 33 away from the cell body 1 , and the mask layer 4 can cover the composite transmission layer 3 on the front and back sides of the cell body 1 .

[0060] During the process of depositing the composite transmission layer 3 on the front and back sides of the battery cell body 1, due to the wrap-around plating phenomenon, the composite transmission layer 3 is also deposited on the side of the battery cell body 1. The composite transmission layer 3 located on the front or back side of the battery cell body 1 is the first composite transmission layer, and the composite transmission layer 3 located on the side of the battery cell body 1 is the second composite transmission layer. Since the second composite transmission layer is generated synchronously when the first composite transmission layer is deposited, the second composite transmission layer and the first composite transmission layer are integrally connected, and the second composite transmission layer covers the four sides of the battery cell body 1.

[0061] If the second composite transmission layer connected to the first composite transmission layer on the front of the cell body 1 and the second composite transmission layer connected to the first composite transmission layer on the back of the cell body 1 are turned on, the conduction between the front and back of the cell body 1 will cause leakage, which will reduce the opening voltage Voc of the cell body 1 and ultimately reduce the photoelectric conversion efficiency of the cell body 1. Therefore, it is necessary to set a mask layer 4 on the composite transmission layer 3 on the front and back of the cell body 1 to remove the composite transmission layer 3 on the side of the cell body 1 and retain the composite transmission layer 3 on the front and back of the cell body 1.

[0062] The steps of preparing the mask layer 4 are: using a mass transfer process, the mask layer 4 is transferred to the front and back of the battery cell body 1. The mask layer 4 can be in the form of a dry film or a liquid. The mask layer 4 can also be a photosensitive or thermosetting insulating material. Including but not limited to covering the battery cell body 1 by pressing, spraying, printing, etc. Then, it is heated and cured to prevent adhesion on the surface and have the function of resisting acid etching chemicals. The thickness of the mask layer 4 formed is 5um to 30um.

[0063] S3. See Appendix Figure 5-8 As shown, the composite transmission layer 3 not covered by the mask layer 4 is removed by a wet etching process;

[0064] Since the second transmission layer 32 has good chemical resistance and is a hard mask, it is difficult to etch it with acid. In the present application, the upper and lower surfaces of the second composite transmission layer 3 are the first transmission layer 31 and the bottom conductive layer 33, respectively. At this time, the bottom conductive layer 33 and the first transmission layer 31 can be etched and removed together with an inorganic acid, an organic acid, or a mixed acid. At this time, because the first transmission layer 31 with poor chemical resistance under the hard mask layer such as SnO2, FTO and SiO2 has been etched and removed, the second transmission layer 32 with good chemical resistance is also peeled off and removed. In this way, the multi-functional indium removal and cost reduction are achieved, the production is easy, the overall continuous production of the battery cell body 1 is matched, the indium poisoning operating environment is removed, and the leakage is isolated to match the copper electroplating process to produce the battery cell body 1 with a side insulation structure, so as to achieve overall efficiency improvement and cost reduction.

[0065] The composite transmission layer 3 not covered by the mask layer 4 is etched with an acidic solution, wherein the acidic solution is an organic acid and / or an inorganic acid selected from any one or more of formic acid, hydrochloric acid, sulfuric acid, and nitric acid. The etching temperature is 20°C to 55°C, the operation time is 1min to 5min, and the spray pressure is 1.5Kg / cm 2 ~5Kg / cm 2 The composite transmission layer 3 and the base layer 2 in the area of ​​the cell body 1 not covered by the mask are etched and removed, thereby obtaining a cell body 1 with a fully insulated or partially insulated side structure.

[0066] See attached Figure 7 and attached Figure 8As shown, in some embodiments, when etching and removing the base layer 2 of the region of the battery cell body 1 not covered by the masking layer 4, appropriate adjustments can be made relative to the process conditions of full etching and removal on the sides. It is achieved that only the range (Te) extending from the center of the thickness (Tt) of the battery cell body 1 to both sides is removed, where 0.1Tt < Te < 0.95Tt. That is, the distance Te between the two side base layers 2 satisfies the following relationship: 0.1Tt < Te < 0.95Tt, and Tt is the thickness of the battery cell body 1. By retaining part of the side base layer 2, the sides of the battery cell body 1 are in a micro-conductive state.

[0067] S4. Through the yellow light pattern transfer process, copper electroplating process, and film stripping and bottom copper etching process, a side-insulated indium-free TCO battery cell body 1 is fabricated. Since the yellow light pattern transfer process, copper electroplating process, and film stripping and bottom copper etching process are conventional techniques in the art and not the inventive points of this application, they will not be elaborated here.

[0068] Embodiment

[0069] The following embodiments more specifically describe the content disclosed in the present invention. These embodiments are only for illustrative purposes, because various modifications and changes within the scope of the content disclosed in the present invention are obvious to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on weight, and all reagents used in the embodiments are commercially available or synthesized according to conventional methods and can be used directly without further treatment, and all instruments used in the embodiments are commercially available.

[0070] "Flush" in this application means that the lengths or widths of the edges of two different structural layers of the battery are almost the same, and the projections of the two different structural layers along the direction perpendicular to the body of the battery almost overlap. "Almost" here means that the deviation between the two can be 0 mm or 0.1 mm or 0.2 mm, or other dimensional deviations. However, generally, the side edges of different structural layers should be on a substantially the same surface visually.

[0071] "Chemical resistance" in this application refers to the ability of a material to resist the erosion of chemical substances.

[0072] Embodiment 1

[0073] An embodiment of the present invention provides a method for preparing a de-indium battery cell, including the following steps:

[0074] S1. Prepare a base layer 2 and a composite transport layer 3 on the front and back of the battery cell body 1.

[0075] A base layer 2 is prepared on the front and back sides of the cell body 1 by a PECVD process, the base layer comprising an intrinsic passivation layer 21 and a microcrystalline silicon layer 22, the intrinsic passivation layer 21 is arranged to fit the cell body 1, the microcrystalline silicon layer 22 is arranged to fit the intrinsic passivation layer 21, the thickness of the intrinsic passivation layer 21 is 5 nm, and the thickness of the microcrystalline silicon layer 32 is 10 nm.

[0076] The composite transmission layer 3 is deposited on the base layer 2 by a PVD deposition process. The composite transmission layer 3 includes a first transmission layer 31 , a second transmission layer 32 and a bottom conductive layer 33 which are arranged in sequence.

[0077] The first transmission layer 31 is located on the side of the substrate 2 away from the cell body 1. The material of the first transmission layer 31 is aluminum-doped zinc oxide (AZO) material. The AZO material includes ZnO and Al2O3, and the weight ratio of ZnO to Al2O3 is 90:10. The first transmission layer 31 is a single-layer structure with a thickness of 5nm.

[0078] The second transmission layer 32 is deposited on the first transmission layer 31. The second transmission layer 32 is arranged on the side of the first transmission layer 31 away from the battery cell body 1. The chemical resistance of the second transmission layer 32 is better than that of the first transmission layer 31. The chemical resistance of the material of the second transmission layer 32 is good, and the material is SnO2. The second transmission layer 32 is a single-layered structure with a thickness of 5nm.

[0079] A bottom conductive layer 33 is deposited on the second transmission layer 32. The bottom conductive layer 33 is arranged on a side of the second transmission layer 32 away from the battery cell body 1. The bottom conductive layer 33 has a thickness of 30 nm and is made of metallic copper.

[0080] During the process of depositing and preparing the composite transmission layer 3, the composite transmission layer 3 is deposited on both sides of the front and back sides of the battery cell body 1. Since the carrier and the back side of the battery cell body 1 abut against each other to support the battery cell body 1, after deposition, the front side of the battery cell body 1 is completely covered with the composite transmission layer 3 to be prepared, and an insulating area 5 is formed on the back side of the battery cell body 1 in the area where the carrier supports and contacts the battery cell body 1.

[0081] S2. A mask layer 4 is provided on the front and back sides of the battery cell body 1. The mask layer 4 is provided on the side of the bottom conductive layer 33 away from the battery cell body 1. The mask layer 4 can cover the composite transmission layer 3 on the front and back sides of the battery cell body 1.

[0082] The steps of preparing the mask layer 4 are: using a dry film to cover and bond the two surfaces of the cell. The operating conditions are 2.5 Kg / cm 2The pressurization process was carried out at a pressure of 30 seconds and a temperature of 35°C, and the resulting coating thickness was 30 um.

[0083] S3, remove the composite transmission layer 3 not covered by the mask layer 4 through a wet etching process; specifically, the cell that has completed the S2 process is loaded into a wet etching device. A mixture of 7.5% hydrochloric acid + 2.5% nitric acid and water is used at an operating temperature of 40°C and an operating time of 120 seconds, with a spray pressure of 2.5Kg / cm 2 The process is to etch and remove the cell base layer and the composite transmission layer not covered by the mask layer 4.

[0084] S4, after washing, an insulating structure is formed. Then, a yellow light pattern transfer process, a copper electroplating process and a film removal bottom copper etching back process are performed to complete and obtain an indium-free TCO cell with side insulation.

[0085] Example 2

[0086] S1. Prepare a base layer 2 and a composite transmission layer 3 on the front and back sides of a battery cell body 1.

[0087] A base layer 2 is prepared on the front and back sides of the cell body 1, and the base layer includes an intrinsic passivation layer 21 and a microcrystalline silicon layer 22. The intrinsic passivation layer 21 is arranged to fit the cell body 1, and the microcrystalline silicon layer 22 is arranged to fit the intrinsic passivation layer 21. The thickness of the intrinsic passivation layer 21 is 120nm, and the thickness of the microcrystalline silicon layer 32 is 30nm.

[0088] The composite transmission layer 3 is deposited on the base layer 2 by the RPD deposition process. The composite transmission layer 3 includes a first transmission layer 31 , a second transmission layer 32 and a bottom conductive layer 33 which are arranged in sequence.

[0089] The first transmission layer 31 is located on the side of the substrate layer 2 away from the cell body 1. The material of the first transmission layer 31 is gallium-doped zinc oxide (GZO) material. The first transmission layer 31 is a multi-layer composite layer structure with a thickness of 120 nm.

[0090] The second transmission layer 32 is deposited on the first transmission layer 31. The second transmission layer 32 is arranged on the side of the first transmission layer 31 away from the battery cell body 1. The chemical resistance of the second transmission layer 32 is better than that of the first transmission layer 31. The chemical resistance of the material of the second transmission layer 32 is good, and the material is fluorine-doped tin oxide. The second transmission layer 32 is a multi-layer composite layered structure with a thickness of 120nm.

[0091] A bottom conductive layer 33 is deposited on the second transmission layer 32. The bottom conductive layer 33 is arranged on a side of the second transmission layer 32 away from the battery cell body 1. The bottom conductive layer 33 has a thickness of 120 nm and is made of metallic copper.

[0092] During the deposition process of preparing the composite transmission layer 3, single-sided preparation is performed, that is, the composite transmission layer 3 on one single side is prepared first, such as the front side of the cell body 1, which is the side not in contact with the carrier; then the cell body 1 is turned over, and the composite transmission layer 3 is prepared on the other single side. Since the composite transmission layer 3 is deposited on the side of the cell body 1 not in contact with the carrier in sequence, the front and back sides of the cell body 1 are fully covered with the composite transmission layer 3.

[0093] S2. A mask layer 4 is provided on the front and back sides of the battery cell body 1. The mask layer 4 is provided on the side of the bottom conductive layer 33 away from the battery cell body 1. The mask layer 4 can cover the composite transmission layer 3 on the front and back sides of the battery cell body 1.

[0094] The steps of preparing the mask layer 4 are: using a dry film to cover and bond the two surfaces of the cell. The operating conditions are 2.5 Kg / cm 2 The pressurization process was carried out at a pressure of 30 seconds and a temperature of 35°C, and the resulting coating thickness was 30 um.

[0095] S3, remove the composite transmission layer 3 not covered by the mask layer 4 through a wet etching process; specifically, the cell that has completed the S2 process is loaded into a wet etching device. A mixture of 5.5% hydrochloric acid + 2.5% formic acid + 1.0% nitric acid and water is used at an operating temperature of 40°C and an operating time of 120 seconds, with a spray pressure of 2.5Kg / cm 2 The process is used to etch and remove the cell base layer and the composite transmission layer that are not covered by the dry film.

[0096] S4, after washing, an insulating structure is formed. Then, a yellow light pattern transfer process, a copper electroplating process and a film removal bottom copper etching back process are performed to complete and obtain an indium-free TCO cell with side insulation.

[0097] Example 3

[0098] An embodiment of the present invention provides a method for preparing an indium-free battery cell, comprising the following steps:

[0099] S1. Prepare a base layer 2 and a composite transmission layer 3 on the front and back sides of a battery cell body 1.

[0100] A base layer 2 is prepared on the front and back sides of the cell body 1 by a PECVD process, the base layer comprising an intrinsic passivation layer 21 and a microcrystalline silicon layer 22, the intrinsic passivation layer 21 is arranged in contact with the cell body 1, the microcrystalline silicon layer 22 is arranged in contact with the intrinsic passivation layer 21, the thickness of the intrinsic passivation layer 21 is 8nm, and the thickness of the microcrystalline silicon layer 32 is 20nm.

[0101] The composite transmission layer 3 is deposited on the base layer 2 by a PVD deposition process. The composite transmission layer 3 includes a first transmission layer 31 , a second transmission layer 32 and a bottom conductive layer 33 which are arranged in sequence.

[0102] The first transmission layer 31 is located on the side of the substrate 2 away from the cell body 1. The material of the first transmission layer 31 is aluminum gallium co-doped zinc oxide material. The first transmission layer 31 is a single layer structure with a thickness of 60nm.

[0103] The second transmission layer 32 is deposited on the first transmission layer 31. The second transmission layer 32 is arranged on the side of the first transmission layer 31 away from the battery cell body 1. The chemical resistance of the second transmission layer 32 is better than that of the first transmission layer 31. The chemical resistance of the material of the second transmission layer 32 is good, and the material is silicon oxide. The second transmission layer 32 is a multi-layer composite layered structure with a thickness of 60nm.

[0104] A bottom conductive layer 33 is deposited on the second transmission layer 32. The bottom conductive layer 33 is arranged on a side of the second transmission layer 32 away from the battery cell body 1. The bottom conductive layer 33 has a thickness of 70 nm and is made of metallic silver.

[0105] During the process of depositing and preparing the composite transmission layer 3, the composite transmission layer 3 is deposited on both sides of the front and back sides of the battery cell body 1. Since the carrier and the back side of the battery cell body 1 abut against each other to support the battery cell body 1, after deposition, the front side of the battery cell body 1 is completely covered with the composite transmission layer 3 to be prepared, and an insulating area 5 is formed on the back side of the battery cell body 1 in the area where the carrier supports and contacts the battery cell body 1.

[0106] S2. A mask layer 4 is provided on the front and back sides of the battery cell body 1. The mask layer 4 is provided on the side of the bottom conductive layer 33 away from the battery cell body 1. The mask layer 4 can cover the composite transmission layer 3 on the front and back sides of the battery cell body 1.

[0107] The steps of preparing the mask layer 4 are: using a dry film to cover and bond the two surfaces of the cell. The operating conditions are 2.5 Kg / cm 2 The pressurization process was carried out at a pressure of 30 seconds and a temperature of 20°C, and the resulting coating thickness was 30 um.

[0108] S3, remove the composite transmission layer 3 not covered by the mask layer 4 through a wet etching process; specifically, the cell that has completed the S2 process is loaded into a wet etching device. A mixture of 7.5% hydrochloric acid + 2.5% nitric acid and water is used at an operating temperature of 40°C and an operating time of 120 seconds, with a spray pressure of 1.5Kg / cm 2 The process is to etch and remove the cell base layer and the composite transmission layer not covered by the mask layer 4.

[0109] S4, after washing, an insulating structure is formed. Then, a yellow light pattern transfer process, a copper electroplating process and a film removal bottom copper etching back process are performed to complete and obtain an indium-free TCO cell with side insulation.

[0110] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. An indium-free battery cell, comprising a battery cell body (1), characterized in that: Further comprising: A composite transmission layer (3), which is disposed on the front and back surfaces of the battery cell body (1); The composite transmission layer (3) includes a first transmission layer (31) and a second transmission layer (32). The first transmission layer (31) is disposed close to the battery cell body (1), and the second transmission layer (32) is disposed on the side of the first transmission layer (31) away from the battery cell body (1). The chemical resistance of the second transmission layer (32) is better than that of the first transmission layer (31).

2. The indium-free battery cell according to claim 1, characterized in that: The material of the first transmission layer (31) is selected from any one or more of aluminum-doped zinc oxide materials, gallium-doped zinc oxide materials, and aluminum-gallium co-doped zinc oxide materials; the first transmission layer (31) is a single layer or a multi-layer composite layer, and the thickness of the first transmission layer (31) is 5 nm to 120 nm.

3. The indium-free battery cell according to claim 1, characterized in that: The material of the second transmission layer (32) is selected from any one or more of tin oxide, silicon oxide, fluorine-doped tin oxide, and boron-doped zinc oxide. The second transmission layer (32) is a single layer or a multi-layer composite layer, and the thickness of the second transmission layer (32) is 5 nm to 120 nm.

4. The indium-free battery cell according to claim 1, characterized in that: The composite transmission layer (3) further includes a bottom conductive layer (32), which is disposed on the side of the second transmission layer (32) away from the battery cell body (1). The thickness of the bottom conductive layer (32) is 30 nm to 120 nm, and the material of the bottom conductive layer (32) is selected from any one or more of gold, silver, platinum, copper, palladium, titanium, nickel, tungsten, bismuth, vanadium, gallium, and rhodium.

5. The indium-free battery cell according to claim 1, characterized in that: The side surface of the composite transmission layer (3) is flush with the side surface of the battery cell body (1).

6. The indium-free battery cell according to claim 1, characterized in that: Further comprising a base layer (2), which includes a front base layer on the front surface of the battery cell body (1), a back base layer on the back surface of the battery cell body (1), and a side base layer on the side surface of the battery cell body (1). There are two side base layers (2), which are integrally connected to the front base layer (2) and the side base layer (2) respectively. The distance Te between the two side base layers (2) satisfies the following relationship: 0.1Tt < Te < 0.95Tt, where Tt is the thickness of the battery cell body (1).

7. The indium-free battery cell according to claim 6, characterized in that: The base layer (2) includes an intrinsic passivation layer (21) and a microcrystalline silicon layer (22). The intrinsic passivation layer (21) is disposed in contact with the battery cell body (1), and the microcrystalline silicon layer (22) is disposed in contact with the intrinsic passivation layer (21). The thickness of the intrinsic passivation layer (21) is 5 nm to 10 nm, and the thickness of the microcrystalline silicon layer (22) is 10 to 30 nm.

8. The method for preparing an indium-free battery cell according to any one of claims 1 to 7, characterized in that: Including the following steps: S1. Prepare a composite transmission layer (3) on the front and back surfaces of the battery cell body (1). The composite transmission layer (3) includes a first transmission layer (31), a second transmission layer (32), and a bottom conductive layer (32) arranged in sequence; S2. Dispose a mask layer (4) on the side of the composite transmission layer (3) away from the battery cell body (1). The mask layer (4) can cover the composite transmission layer (3) on the front and back surfaces of the battery cell body (1); S3, removing the composite transmission layer (3) not covered by the mask layer (4) through a wet etching process; S4. Through yellow light pattern transfer process, copper electroplating process and film removal bottom copper etching back process, an indium-free battery cell with one side insulated is produced.

9. The method for preparing an indium-free battery cell according to claim 8, characterized in that: In S1, during the process of depositing the composite transmission layer (3), the composite transmission layer (3) is deposited on both sides of the front and back sides of the battery cell body (1) at the same time, so that one side of the battery cell body (1) is completely covered with the prepared composite transmission layer (3), and on the other side of the battery cell body (1), an insulating area (5) is formed in the area where the carrier supports and contacts the battery cell body (1).

10. The method for preparing an indium-free battery cell according to claim 8, characterized in that: In S1, during the process of depositing the composite transmission layer (3), the composite transmission layer (3) is first prepared on one single side, which is the side that does not contact the carrier; then the battery cell body (1) is turned over, and the composite transmission layer (3) is prepared on the other single side, so that the front and back sides of the battery cell body (1) are completely covered with the prepared composite transmission layer (3).

11. The method for preparing an indium-free battery cell according to claim 8, characterized in that: In S3, an acidic solution is used to etch the composite transmission layer (3) not covered by the mask layer (4), and the acidic solution is an organic acid solution or an inorganic acid solution or a mixed solution of an organic acid and an inorganic acid.

12. The method for preparing an indium-free battery cell according to claim 11, characterized in that: In S3, the acidic solution is selected from any one or more of formic acid, hydrochloric acid, sulfuric acid, and nitric acid.

13. The method for preparing an indium-free battery cell according to claim 8, characterized in that: In S3, the etching temperature is 20℃~55℃, the operation time is 1min~5min, and the spray pressure is 1.5Kg / cm 2 ~5Kg / cm 2 .

14. The method for preparing an indium-free battery cell according to claim 8, characterized in that: In S3, the part or all of the base layer (2) not covered by the mask layer (4) is removed by a wet etching process.