Pole piece insulation treatment method and pole piece manufacturing equipment

By infiltrating insulating slurry into the cut edges of pole piece coils to form a protective layer, the method addresses burr-induced short circuits, enhancing battery reliability and performance.

CN119069648AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310627881.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

Burr formation during the cutting of current collectors in battery manufacturing poses a risk of internal short circuits, compromising battery reliability.

Method used

A method involving cutting pole pieces into sub-pieces, rolling them into coils, and infiltrating the cut edges with insulating slurry to form a protective layer, ensuring the burrs are shielded and reducing the risk of short circuits.

Benefits of technology

The insulating layer effectively shields burrs, enhancing battery cell reliability by preventing piercings through the isolation membrane, thus improving overall battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069648A_ABST
    Figure CN119069648A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a pole piece insulation treatment method and pole piece manufacturing equipment. The pole piece insulation treatment method comprises the following steps: slitting a pole piece into a plurality of sub pole pieces; the sub-pole pieces are wound to form a pole piece coiled material, and the pole piece coiled material comprises a first end face formed by the slitting edges of the sub-pole pieces; the first end face is arranged to face insulating slurry; and infiltrating the first end face with the insulating slurry to form an insulating layer which at least covers a current collector of the sub-pole piece and burrs generated after the current collector is cut. The pole piece manufactured according to the technical scheme provided by the invention can improve the reliability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a pole piece insulation processing method and pole piece manufacturing equipment. Background Art

[0002] Energy conservation and emission reduction are the key to the sustainable development of the automobile industry. Electric vehicles have become an important part of the sustainable development of the automobile industry due to their advantages in energy conservation and environmental protection. For electric vehicles, battery technology is an important factor in their development.

[0003] During the manufacturing process of batteries, the reliability of batteries is an issue that cannot be ignored. Therefore, how to improve the reliability of batteries is a technical problem that needs to be solved urgently in battery technology. Summary of the invention

[0004] The present application provides a pole piece insulation processing method and a pole piece manufacturing device, and the manufactured pole piece can improve the reliability of the battery.

[0005] This application is achieved through the following technical solutions:

[0006] In a first aspect, an embodiment of the present application provides a method for insulating a pole piece, comprising: cutting a pole piece into a plurality of sub-pole pieces; rolling up the sub-pole pieces to form a pole piece roll, wherein the pole piece roll comprises a first end face formed by the cut edges of the sub-pole pieces; arranging the first end face facing an insulating slurry; and infiltrating the first end face with the insulating slurry to form an insulating layer that at least covers the current collectors of the sub-pole pieces and burrs generated after the current collectors are cut.

[0007] According to the pole piece insulation processing method of the embodiment of the present application, the insulating slurry is infiltrated into the cut edge of the sub-pole piece, thereby forming an insulating layer on the first end face of the pole piece coil. The insulating layer can cover the current collector and the burrs generated after the current collector is cut, thereby shielding the burrs and reducing the risk of the burrs piercing the isolation membrane and causing an internal short circuit in the battery cell. The operation is simple and can improve the reliability of the battery cell.

[0008] According to some embodiments of the present application, the step of infiltrating the first end surface with the insulating slurry includes: stirring the insulating slurry so that the surging insulating slurry infiltrates the first end surface.

[0009] In the above scheme, the insulating slurry is stirred so that the surging insulating slurry infiltrates the first end surface, thereby reducing the risk of bubbles between the insulating slurry and the first end surface after the insulating slurry infiltrates the first end surface, thereby facilitating improving the infiltration effect of the insulating slurry.

[0010] According to some embodiments of the present application, before the insulating slurry is stirred, the first end surface is not in contact with the insulating slurry.

[0011] In the above solution, before the insulating slurry is stirred, the first end surface is not in contact with the insulating slurry, so as to reduce the risk of the insulating slurry infiltrating the pole piece coil and causing the two adjacent circles of pole pieces to stick together.

[0012] According to some embodiments of the present application, the stirring of the insulating slurry includes: stirring the insulating slurry so that the insulating slurry forms waves, and the crest of the wave is higher than the first end surface.

[0013] In the above scheme, the insulating slurry is stirred to form waves, and the crest of the wave is higher than the first end face, so that the insulating slurry can infiltrate the first end face. By controlling the crest of the wave, the infiltration amount of the insulating slurry and the pole piece coil can be adjusted.

[0014] According to some embodiments of the present application, before the insulating slurry is stirred, the distance between the first end surface and the insulating slurry is H1, and after the insulating slurry is stirred to form the wave, the peak height of the wave is H2, satisfying 1mm≤H2-H1≤5mm.

[0015] In the above scheme, (H2-H1) can be the size of the wave exceeding the first end face, that is, the size of the insulating slurry infiltrating the sub-pole piece in the vertical direction, which can determine the thickness of the insulating layer attached to the first end face. The peak height H2 and the distance H1 between the first end face and the insulating slurry satisfy the above relationship, and can control the thickness of the insulating layer formed on the first end face to meet the shielding of burrs. If the value of (H2-H1) is small (such as less than 1mm), the thickness of the insulating layer is thin, the burrs are easy to pierce the insulating layer, and the insulation effect is poor; if the value of (H2-H1) is large (such as greater than 5mm), the height of the insulating slurry surges is high, the insulating slurry is easy to penetrate between the two adjacent layers of sub-pole pieces, and it is easy to cause the two adjacent layers of sub-pole pieces to stick together. When the pole piece coil is unfolded, it is easy to cause the insulating layer to detach from the first end face, resulting in insulation failure.

[0016] According to some embodiments of the present application, 2mm≤H2-H1≤4mm.

[0017] In the above scheme, compared with H2-H1<2mm, when H2-H1≥2mm, the thickness of the insulating layer formed by the insulating slurry on the first end face is thicker, the insulating layer has a better shielding effect on the burrs, and the insulation effect is higher; compared with H2-H1>4mm, when H2-H1≤4mm, the height of the insulating slurry surge is lower, and the insulating slurry is not easy to enter between the two adjacent layers of sub-pole pieces. While the insulating layer has a better shielding effect on the burrs, the insulating layer is lowered to make the two adjacent layers of sub-pole pieces adhere.

[0018] According to some embodiments of the present application, when the insulating slurry is stirred, the pole piece coil does not rotate.

[0019] In the above scheme, since the insulating slurry is located below the pole piece coil, if the pole piece coil is rotated, it is easy for the pole piece coil to separate from the winding roller and fall into the insulating slurry. In this embodiment, the pole piece coil does not rotate, which can reduce the risk of the pole piece coil separating from the winding roller.

[0020] According to some embodiments of the present application, the stirring of the insulating slurry includes: stirring the insulating slurry by rotating a stirring member, wherein the rotation axis of the stirring member is colinear with the central axis of the pole piece coil.

[0021] In the above scheme, the insulating slurry is surged by rotating the agitator, and the rotation axis of the agitator is colinear with the central axis of the pole piece coil, so that the surged insulating slurry can evenly cover the first end surface and is easy to operate.

[0022] According to some embodiments of the present application, an extension direction of the agitator intersects with a central axis of the pole piece coil.

[0023] In the above scheme, the extension direction of the agitator intersects with the central axis of the pole piece coil. When the extension direction of the agitator is parallel to the first end face, the extension direction of the agitator can be parallel to the radial direction of the first end face, so that the agitator can have a larger overlapping area with the first end face in the radial direction of the first end face, so that when the agitator stirs the insulating slurry, the surging insulating slurry can cover the inner and outer circles of the first end face, thereby improving the coating efficiency of the insulating slurry on the first end face.

[0024] According to some embodiments of the present application, along the extension direction of the central axis of the pole piece coil, the projection of the stirring member is located on one side of the central axis of the pole piece coil.

[0025] In the above scheme, the extension direction of the central axis of the pole piece coil is used as the projection direction, and the projection of the agitator on the plane perpendicular to the central axis of the pole piece coil is located on one side of the central axis of the pole piece coil. The space occupied by the agitator in the radial direction of the pole piece coil can be smaller, which is convenient for the layout of the insulating parts, reduces the space occupied by the agitator, and reduces the risk of interference between the agitator and the winding roller on which the pole piece coil is set.

[0026] According to some embodiments of the present application, along the extension direction of the central axis of the pole piece coil, both ends of the projection of the agitator along the extension direction of the agitator exceed the inner circle and the outer circle of the first end surface.

[0027] In the above scheme, the two ends of the projection of the agitator along the extension direction of the agitator exceed the inner circle and the outer circle of the first end face, that is, the agitator has a large overlapping area with the first end face in the radial direction of the first end face. During the rotation of the agitator, the surging insulating slurry can cover the inner circle and the outer circle of the first end face. The insulating slurry can be infiltrated into the first end face once by rotating the agitator one circle, and the infiltration efficiency is high.

[0028] According to some embodiments of the present application, before the insulating slurry is stirred by rotating the stirring member, the stirring member is located in the insulating slurry and the stirring member does not exceed the liquid surface of the insulating slurry.

[0029] In the above solution, the stirring member does not exceed the liquid surface of the insulating slurry, which can reduce the risk of interference between the stirring member and the winding roller of the winding sub-pole piece.

[0030] According to some embodiments of the present application, after the wetting of the first end surface of a pole piece coil is completed, the stirring speed of the insulating slurry is reduced, a pole piece coil to be insulated is replaced, and the stirring of the insulating slurry is repeated.

[0031] In the above scheme, after the first end surface of a pole piece coil is wetted, the stirring speed of the insulating slurry is reduced so that the insulating slurry tends to be stationary, so as to facilitate the replacement of the pole piece coil to be insulated, and then the insulating slurry is repeatedly stirred so that the insulating slurry can wet the first end surface, thereby reducing the risk of the insulating slurry splashing to other areas when the pole piece coil is replaced.

[0032] In the second aspect, the embodiment of the present application provides a pole piece manufacturing device, including: a slitting device, a winding device, a container, a positioning device and a stirring device. The slitting device is used to slit the pole piece into a plurality of sub-pole pieces; the winding device is used to wind up the sub-pole pieces to form a pole piece coil, and the pole piece coil includes a first end face formed by the slitting edges of the sub-pole pieces; the container is used to contain insulating slurry; the positioning device is used to position the pole piece coil; the stirring device is used to stir the insulating slurry in the container so that the surging insulating slurry infiltrates the first end face to form an insulating layer that at least covers the current collector of the sub-pole piece and the burrs generated after the current collector is cut.

[0033] According to the pole piece manufacturing equipment of the embodiment of the present application, the pole piece is cut into a plurality of sub-pole pieces by a slitting device, the winding device can wind up the sub-pole pieces to form a pole piece coil, and the positioning device can realize the positioning of the pole piece coil, so that the insulating slurry stirred by the stirring device can infiltrate the first end surface, and form an insulating layer on the first end surface to cover the current collector and the burrs generated after the current collector is cut. The manufactured pole piece can reduce the risk of burrs piercing the isolation membrane and causing internal short circuit of the battery cell, and can improve the reliability of the battery cell.

[0034] According to some embodiments of the present application, the stirring device includes a stirring member and a driving member, the stirring member is arranged in the insulating slurry, the driving member is transmission-connected to the stirring member, and the driving member is used to drive the stirring member to rotate relative to the container to surge the insulating slurry.

[0035] In the above solution, the agitator, driven by the driving member, can cause the insulating slurry in the container to surge, so that the surged insulating slurry infiltrates the first end surface, and then forms an insulating layer on the first end surface. The structure is simple and the operation is convenient.

[0036] According to some embodiments of the present application, the rotation axis of the agitator is colinear with the central axis of the container.

[0037] In the above scheme, the rotation axis of the agitator is colinear with the central axis of the container, so that the pole piece coil is positioned in the container according to the rotation axis of the agitator.

[0038] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 A schematic flow chart of a pole piece insulation treatment method provided in some embodiments of the present application;

[0041] Figure 2 A schematic diagram of the state of pole piece cutting provided in some embodiments of the present application;

[0042] Figure 3 A schematic diagram of a first end surface provided for some embodiments of the present application;

[0043] Figure 4 A schematic diagram of placing a pole sheet coil into a container provided in some embodiments of the present application;

[0044] Figure 5 A schematic diagram of the surging insulating slurry infiltrating the first end surface provided in some embodiments of the present application;

[0045] Figure 6 A schematic block diagram of the structure of a pole piece manufacturing device provided in some embodiments of the present application;

[0046] Figure 7 A schematic diagram of the structure of a pole piece manufacturing device provided in some embodiments of the present application.

[0047] Icons: 100-slitting device; 1-pole piece; 11-sub-pole piece; 2-pole piece coil; 21-first end face; 200-winding device; 20-winding roller; 300-container; 31-wave; 400-positioning device; 41-positioning fixture; 42-fixed frame; 500-stirring device; 51-stirring member; 52-driving member; 53-turntable; 600-detection device. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0049] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned drawings and any variations thereof are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship.

[0050] Reference to "embodiments" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application may be combined with other embodiments.

[0051] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "attached" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0052] The term "and / or" in this application is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this application generally indicates that the associated objects before and after are in an "or" relationship.

[0053] The term "multiple" as used in this application refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple sheets" refers to more than two sheets (including two sheets).

[0054] In some embodiments, the battery may be a battery module. When there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module.

[0055] In some embodiments, the battery may be a battery pack, which includes a case and battery cells, wherein the battery cells or battery modules are accommodated in the case.

[0056] In some embodiments, the box body can be used as a part of the chassis structure of the vehicle. For example, part of the box body can become at least a part of the floor of the vehicle, or part of the box body can become at least a part of the cross beam and longitudinal beam of the vehicle.

[0057] In some embodiments, the battery may be an energy storage device, which includes an energy storage container, an energy storage cabinet, and the like.

[0058] In the embodiment of the present application, the battery cell may be a secondary battery. A secondary battery refers to a battery cell that can be continuously used by activating active materials by charging after the battery cell is discharged.

[0059] The battery cells may be, but are not limited to, lithium ion batteries, sodium ion batteries, sodium lithium ion batteries, lithium metal batteries, sodium metal batteries, lithium sulfur batteries, magnesium ion batteries, nickel hydrogen batteries, nickel cadmium batteries, lead storage batteries, etc.

[0060] A battery cell generally includes an electrode assembly. The electrode assembly includes a positive electrode, a negative electrode, and a separator. During the charge and discharge process of the battery cell, active ions (such as lithium ions) are embedded and removed between the positive electrode and the negative electrode. The separator is set between the positive electrode and the negative electrode to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through.

[0061] In some embodiments, the positive electrode may be a positive electrode sheet, and the positive electrode sheet may include a positive electrode current collector and a positive electrode active material disposed on at least one surface of the positive electrode current collector.

[0062] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material is disposed on either or both of the two facing surfaces of the positive electrode current collector.

[0063] As an example, the positive electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, aluminum with a silver-plated surface, stainless steel with a silver-plated surface, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium, etc., may be used. The composite current collector may include a polymer material base and a metal layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).

[0064] As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used.

[0065] In some embodiments, the negative electrode may be a negative electrode sheet, and the negative electrode sheet may include a negative electrode current collector.

[0066] As an example, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, aluminum with a silver-plated surface, stainless steel with a silver-plated surface, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium, etc. may be used.

[0067] In some embodiments, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode active material is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0068] As an example, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0069] In some embodiments, the separator is a separator. The present application has no particular limitation on the type of separator, and any known separator with a porous structure having good chemical stability and mechanical stability can be selected.

[0070] As an example, the main material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, and ceramic. The separator can be a single-layer film or a multi-layer composite film, without special restrictions. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without special restrictions. The separator can be a separate component located between the positive and negative electrodes, or it can be attached to the surface of the positive and negative electrodes.

[0071] In some embodiments, the electrode assembly is a wound structure, wherein the positive electrode sheet and the negative electrode sheet are wound into the wound structure.

[0072] In some embodiments, the electrode assembly is a laminate structure.

[0073] In some embodiments, the battery cell may include a housing. The housing is used to encapsulate components such as the electrode assembly and the electrolyte. The housing may be a steel housing, an aluminum housing, a plastic housing (such as polypropylene), a composite metal housing (such as a copper-aluminum composite housing), or an aluminum-plastic film.

[0074] The development of battery technology must take into account many design factors at the same time, such as energy density, discharge capacity, charge and discharge rate and other performance parameters. In addition, battery reliability must also be considered.

[0075] During the battery manufacturing process, the manufacturing process of the pole piece includes a slitting process. The pole piece is usually a continuous strip structure with a certain width. The pole piece is cut into multiple sub-pole pieces through the slitting process. The cutting edge of the sub-pole piece is formed with burrs, which are generated after the current collector is cut. When the pole piece forms a battery cell, the burrs are easy to pierce the isolation membrane, thereby causing an internal short circuit in the battery cell, which can cause fire, explosion, etc. in severe cases, making the reliability of the battery cell poor.

[0076] In view of this, in order to solve the problem that burrs pierce the isolation membrane and cause internal short circuit of the battery cell, resulting in poor reliability of the battery cell, the embodiment of the present application provides a technical solution. After the pole piece is cut into multiple sub-pole pieces, the sub-pole pieces are rolled up to form a pole piece coil, and the pole piece coil is placed in a container containing insulating slurry, the insulating slurry is soaked in the first end surface, and an insulating layer covering the burrs is formed on the first end surface. The manufactured pole piece can improve the reliability of the battery cell.

[0077] By adopting the above-mentioned technical scheme, the insulating slurry is infiltrated into the first end face, that is, the insulating slurry is infiltrated into all the cut edges of the sub-pole pieces to form an insulating layer on the first end face, and the insulating layer at least covers the current collector and the burrs generated after the current collector is cut, and the insulating layer covers a part of the active material layer to shield the burrs. After the manufactured pole pieces constitute battery cells, the burrs are not easy to pierce the isolation membrane due to the shielding of the insulating layer, thereby reducing the risk of the burrs piercing the isolation membrane and causing internal short circuit of the battery cell, so that the battery cell can have higher reliability.

[0078] The following describes the pole piece insulation processing method of the embodiment of the present application in conjunction with the accompanying drawings.

[0079] Please refer to Figures 1 to 5 , Figure 1 A schematic flow chart of a method for insulating a pole piece provided in some embodiments of the present application. Figure 2 A schematic diagram of the state of pole piece cutting provided in some embodiments of the present application, Figure 3 A schematic diagram of a first end surface provided in some embodiments of the present application, Figure 4 A schematic diagram of placing a pole sheet coil into a container provided in some embodiments of the present application, Figure 5 A schematic diagram of a first end surface infiltrated by a surging insulating slurry provided in some embodiments of the present application. According to some embodiments of the present application, an insulation treatment method for a pole piece is provided, and the insulation treatment method for a pole piece includes:

[0080] S110, cutting the pole piece 1 into a plurality of sub-pole pieces 11;

[0081] S120, rolling up the sub-pole sheet 11 to form a pole sheet coil 2, wherein the pole sheet coil 2 includes a first end surface 21 formed by the cut edges of the sub-pole sheet 11;

[0082] S130, placing the first end surface 21 facing the insulating slurry;

[0083] S140 , infiltrating the first end surface 21 with an insulating slurry to form an insulating layer that at least covers the current collector of the sub-electrode sheet 11 and burrs generated after the current collector is cut.

[0084] The pole piece 1 is cut into a plurality of sub-pole pieces 11, which can improve the manufacturing efficiency of the pole piece 1. After the pole piece 1 is cut, two sub-pole pieces 11, three sub-pole pieces 11 or more than three sub-pole pieces 11 can be formed.

[0085] The pole piece 1 is usually a continuous strip structure. The pole piece 1 is cut into sub-pole pieces 11 . The sub-pole pieces 11 are rolled up on a winding roller 20 to form a pole piece coil 2 for the convenience of subsequent process operations.

[0086] The first end face 21 is an end face formed by the cut edge of the sub-electrode piece 11. Figure 3The first end surface 21 as a whole can be an annular surface, and the first end surface 21 has an inner ring 211 and an outer ring 212 , wherein the inner ring 211 is close to the winding roller 20 and the outer ring 212 is far away from the winding roller 20 .

[0087] In step "S130, setting the first end surface 21 facing the insulating slurry", the pole piece coil 2 can be positioned by a positioning device to fix the relative position of the pole piece coil 2 and the insulating slurry in the container 300. In this step, the first end surface 21 is set to face the insulating slurry, and the first end surface 21 is parallel to the liquid surface of the insulating slurry in the container 300, so that the insulating slurry covers the first end surface 21 evenly. In this step, the pole piece coil 2 can be located outside the container 300 or inside the container 300.

[0088] In the step “S140, soaking the first end face 21 with the insulating slurry”, the first end face 21 can be directly immersed in the insulating slurry, or the insulating slurry can be stirred by a stirring device to make the insulating slurry surge, and the surged insulating slurry can soak the first end face 21, so that the insulating slurry forms an insulating layer on the first end face 21, and the insulating layer at least covers the current collector and the burrs generated after the current collector is cut. In the direction perpendicular to the first end face 21, the projection of the burr partially overlaps with the active material layer. When the insulating slurry soaks the first end face 21, the insulating slurry adheres to the current collector, the active material layer and the burrs, so that the formed insulating layer can cover the current collector and the burrs.

[0089] The insulating slurry may include a solid insulating material, a binder and a solvent. The solid insulating material may be selected from at least one of BaSO4, CaSiO3, γ-AlOOH, CaSiO4 and polytetrafluoroethylene. The binder may be selected from at least one of polyvinylidene fluoride binder, styrene-butadiene rubber binder, polyetherimide binder, sodium polyacrylate binder, polytetrafluoroethylene binder, acrylate binder and carboxymethyl cellulose binder. The solvent is selected according to the properties of the binder. When the binder is an aqueous binder, an aqueous solvent (such as distilled water, etc.) may be selected; when the binder is an oily binder, an oily solvent (such as N-methylpyrrolidone, etc.) may be selected.

[0090] According to the pole piece insulation processing method of the embodiment of the present application, the insulating slurry is infiltrated into the cut edge of the sub-pole piece 11, so as to form an insulating layer on the first end surface 21 of the pole piece coil 2. The insulating layer can cover the current collector and the burrs generated after the current collector is cut, and play a shielding role on the burrs, thereby reducing the risk of the burrs piercing the isolation membrane and causing an internal short circuit in the battery cell. The operation is simple and can improve the reliability of the battery cell.

[0091] According to some embodiments of the present application, infiltrating the first end surface 21 with the insulating slurry includes: stirring the insulating slurry so that the surging insulating slurry infiltrates the first end surface 21 .

[0092] In the above scheme, the insulating slurry is stirred so that the surging insulating slurry infiltrates the first end surface 21, thereby reducing the risk of bubbles between the insulating slurry and the first end surface 21 after the insulating slurry infiltrates the first end surface 21, thereby improving the infiltration effect of the insulating slurry.

[0093] Please refer to Figure 4 According to some embodiments of the present application, before the insulating slurry is stirred, the first end surface 21 is not in contact with the insulating slurry.

[0094] In the step “ S130 , arranging the first end surface 21 to face the insulating slurry”, a portion of the pole piece 1 that is insulated is located in the container 300 , wherein the first end surface 21 is in the container 300 .

[0095] If the first end face 21 is in contact with the insulating slurry, when the insulating slurry is stirred, the contact area between the insulating slurry and the sub-pole piece 11 in the vertical direction is large, and the insulating slurry is easy to penetrate between two adjacent circles of pole pieces 11, thereby causing the two adjacent circles of pole pieces 11 to adhere to each other. After the insulating slurry solidifies, when the sub-pole piece 11 is unfolded, it is easy to cause the insulating layer attached to the first end face 21 to separate from the sub-pole piece 11, lose coverage of the burrs, and cause insulation failure.

[0096] In the above scheme, before the insulating slurry is stirred, the first end face 21 is not in contact with the insulating slurry in the container 300. After the insulating slurry is stirred, the surging insulating slurry is used to infiltrate the first end face 21, and the amount of insulating slurry attached to the first end face 21 is controlled to reduce the risk of the insulating slurry infiltrating the pole piece coil 2 and causing the two adjacent circles of pole pieces 11 to stick together.

[0097] According to some embodiments of the present application, in step "S130, arranging the first end surface 21 facing the insulating slurry", the pole piece coil 2 may be positioned by a positioning device to determine the distance between the first end surface 21 and the liquid surface of the insulating slurry. For example, the pole piece coil 2 may be suspended above the insulating slurry by the positioning device so that the first end surface 21 does not contact the liquid surface of the insulating slurry.

[0098] In some embodiments, while the insulating slurry is being stirred, the distance between the first end surface 21 and the liquid surface of the insulating slurry is adjusted to ensure that the surging insulating slurry can infiltrate the first end surface 21 .

[0099] Please refer to Figure 5 According to some embodiments of the present application, stirring the insulating slurry includes: stirring the insulating slurry so that the insulating slurry forms a wave 31 , and the crest of the wave 31 is higher than the first end surface 21 .

[0100] When the insulating slurry is stirred, the surging insulating slurry forms waves 31 , the crest of which is higher than the first end surface 21 , so that the waves 31 can cover the first end surface 21 , so that the insulating slurry can infiltrate the first end surface 21 and form an insulating layer on the first end surface 21 .

[0101] When the insulating slurry is stirred, the waves 31 can cover the entire first end surface 21 , so that the insulating slurry covers the first end surface 21 evenly.

[0102] In some embodiments, the insulating slurry can be stirred by a stirring member, and the length of the stirring member can be greater than or equal to the distance between the inner circle and the outer circle of the first end surface 21, so that the formed waves 31 cover the inner circle and the outer circle of the first end surface 21.

[0103] In the above scheme, the insulating slurry is stirred to form a wave 31, and the crest of the wave 31 is higher than the first end face 21, so that the insulating slurry can infiltrate the first end face 21. By controlling the crest of the wave 31, the wetting amount of the insulating slurry and the pole piece coil 2 can be adjusted.

[0104] Please refer to Figure 4 and Figure 5 According to some embodiments of the present application, before stirring the insulating slurry, the distance between the first end surface 21 and the insulating slurry is H1. After stirring the insulating slurry to form a wave 31, the peak height of the wave 31 is H2, satisfying 1mm≤H2-H1≤5mm.

[0105] Before stirring the insulating slurry, the distance between the first end face 21 and the insulating slurry can be measured by a distance meter. For example, a distance meter is set on the positioning device that clamps the electrode sheet coil 2, and the distance between the distance meter and the first end face 21 is preset. After the electrode sheet coil 2 is positioned in the container 300, the distance between the first end face 21 and the insulating slurry is detected.

[0106] The crest height of the wave 31 may be the distance between the highest point of the wave 31 and the liquid surface of the insulating slurry when it is stationary, and may be measured by a detection device (such as a distance meter). For example, after the insulating slurry is stirred, the distance meter detects the distance between the highest point of the insulating slurry and the distance meter, and the crest height of the wave 31 is obtained by comparing the distance between the distance meter and the insulating slurry when it is stationary.

[0107] (H2-H1) may be the dimension of the wave 31 exceeding the first end surface 21 , that is, the dimension of the insulating paste wetting the sub-pole piece 11 in the vertical direction, which can determine the thickness of the insulating layer attached to the first end surface 21 .

[0108] If the value of (H2-H1) is small (such as less than 1mm), the thickness of the insulating layer is thinner, the burrs are easy to pierce the insulating layer, and the insulation effect is poor; if the value of (H2-H1) is large (such as greater than 5mm), the height of the insulating slurry surges is high, and the insulating slurry is easy to penetrate between the two adjacent layers of sub-pole sheets 11, which is easy to cause the two adjacent layers of sub-pole sheets 11 to stick together. When the electrode sheet roll 2 is unfolded, it is easy to cause the insulating layer to detach from the first end face 21, resulting in insulation failure.

[0109] The peak height H2 and the distance H1 between the first end surface 21 and the insulating paste satisfy the above relationship (1 mm ≤ H2 − H1 ≤ 5 mm), and the thickness of the insulating layer formed on the first end surface 21 can be controlled to meet the requirements of shielding the burrs.

[0110] According to some embodiments of the present application, 2mm≤H2-H1≤4mm.

[0111] Compared with H2-H1<2mm, when H2-H1≥2mm, the thickness of the insulating layer formed by the insulating slurry on the first end surface 21 is thicker, the insulating layer has a better shielding effect on the burrs, and the insulating effect is higher.

[0112] Compared with H2-H1>4mm, when H2-H1≤4mm, the height of the insulating paste surges is lower, and the insulating paste is not easy to enter between two adjacent layers of sub-pole pieces 11. While the insulating layer has a better shielding effect on burrs, the insulating layer is lowered to make the two adjacent layers of sub-pole pieces 11 adhere to each other.

[0113] According to some embodiments of the present application, when the insulating slurry is stirred, the pole piece coil 2 does not rotate.

[0114] Since the insulating paste is located below the pole sheet coil 2, if the pole sheet coil 2 is rotated, the pole sheet coil 2 is easily separated from the winding roller 20 and falls into the insulating paste. In this embodiment, the pole sheet coil 2 does not rotate, which can reduce the risk of the pole sheet coil 2 separating from the winding roller 20.

[0115] According to some embodiments of the present application, stirring the insulating slurry includes: stirring the insulating slurry by rotating a stirring member 51 , wherein the rotation axis of the stirring member 51 is colinear with the central axis P of the pole piece coil 2 .

[0116] When the insulating slurry is stirred by rotating the stirring member 51, the rotation speed of the stirring member 51 affects the crest height of the wave 31. The faster the rotation speed of the stirring member 51, the higher the crest height of the wave 31; conversely, the slower the rotation speed of the stirring member 51, the lower the crest height of the wave 31.

[0117] By rotating the agitator 51, the insulating slurry can be agitated so that the insulating slurry surges, and the surged insulating slurry forms waves 31, and the waves 31 move along the moving trajectory of the agitator 51. The central axis P of the pole piece coil 2 is collinear with the central axis of the first end face 21, and the rotation axis of the agitator 51 is collinear with the central axis P of the pole piece coil 2. The moving trajectory of the agitator 51 can be a circle around the central axis P of the pole piece coil 2. When the waves 31 formed by the insulating slurry move along the moving trajectory of the agitator 51, the insulating slurry can cover the first end face 21 in the circumferential direction of the first end face 21, so as to achieve the infiltration of the insulating slurry on the first end face 21.

[0118] In some embodiments, the agitator 51 may be a plate-shaped structure, so that the agitator 51 can drive more insulating slurry, so that the surging insulating slurry can infiltrate the first end surface 21 .

[0119] In the above scheme, the insulating slurry is surged by rotating the agitator 51, and the rotation axis of the agitator 51 is colinear with the central axis P of the pole piece coil 2, so that the surged insulating slurry can evenly cover the first end surface 21 and the operation is convenient.

[0120] According to some embodiments of the present application, the extension direction of the agitator 51 intersects with the central axis P of the pole piece coil 2 .

[0121] The agitator 51 can be parallel to the first end face 21 so that the waves 31 formed by the agitator 51 stirring the insulating slurry cover the inner and outer circles of the first end face 21, and the insulating slurry can be evenly adhered to the first end face 21, that is, the thickness of the insulating layer on the first end face 21 can be made uniform.

[0122] In the above scheme, the extension direction of the agitator 51 intersects with the central axis P of the pole piece coil 2. When the extension direction of the agitator 51 is parallel to the first end face 21, the extension direction of the agitator 51 can be parallel to the radial direction of the first end face 21, so that the agitator 51 can have a larger overlapping area with the first end face 21 in the radial direction of the first end face 21, so that when the agitator 51 stirs the insulating slurry, the surging insulating slurry can cover the inner and outer circles of the first end face 21, thereby improving the coating efficiency of the insulating slurry on the first end face 21.

[0123] Please refer to Figure 5 According to some embodiments of the present application, along the extension direction of the central axis P of the pole piece coil 2 , the projection of the agitator 51 is located on one side of the central axis P of the pole piece coil 2 .

[0124] Taking the extension direction of the central axis P of the pole piece roll 2 as the projection direction, the projection of the agitator 51 on the plane perpendicular to the central axis P of the pole piece roll 2 is located on one side of the axial axis of the pole piece roll 2, that is, the agitator 51 does not exceed the central axis P of the pole piece roll 2.

[0125] In the above scheme, the projection of the agitator 51 is located on one side of the central axis P of the pole piece coil 2, and the space occupied by the agitator 51 in the radial direction of the pole piece coil 2 can be smaller, which is convenient for the layout of insulating parts, reduces the space occupied by the agitator 51, and reduces the risk of interference between the agitator 51 and the winding roller 20 on which the pole piece coil 2 is set.

[0126] According to some embodiments of the present application, along the extension direction of the central axis P of the pole piece coil 2 , both ends of the projection of the agitator 51 along the extension direction of the agitator 51 exceed the inner circle and the outer circle of the first end surface 21 .

[0127] The first end surface 21 can be regarded as an annular surface. The first end surface 21 has an inner circle and an outer circle. The inner circle is close to the winding roller 20 of the sub-pole piece 11 , and the outer circle is far away from the winding roller 20 of the sub-pole piece 11 .

[0128] The agitator 51 may be a plate-like structure, the agitator 51 may be a rectangular parallelepiped, and the extension direction of the agitator 51 may be the length direction of the agitator 51. The two ends of the projection of the agitator 51 along the extension direction of the agitator 51 may exceed the inner circle and the outer circle of the first end surface 21, and the two ends of the agitator 51 in the length direction may exceed the inner circle and the outer circle of the first end surface 21.

[0129] For example, in an embodiment where the projection of the agitator 51 is located on one side of the central axis P of the pole piece coil 2 along the extension direction of the central axis P of the pole piece coil 2, the agitator 51 is located on one side of the central axis P of the pole piece coil 2, and both ends of the projection of the agitator 51 along the extension direction of the agitator 51 exceed the inner circle and the outer circle of the first end face 21, so that the agitator 51 can cover the inner circle and the outer circle of the first end face 21, and when the agitator 51 stirs the insulating slurry to surge, the waves 31 formed by the insulating slurry can cover the inner circle and the outer circle of the first end face 21.

[0130] For example, in some embodiments, along the extension direction of the central axis P of the pole piece roll 2, the projection of the agitator 51 can be located on both sides of the central axis P of the pole piece roll 2, and the projection of the agitator 51 at both ends of the extension direction of the agitator 51 can also exceed the inner circle and outer circle of the first end face 21. At this time, the length of the agitator 51 can be greater than or equal to the diameter of the pole piece roll 2.

[0131] In the above scheme, the two ends of the projection of the agitator 51 along the extension direction of the agitator 51 exceed the inner circle and the outer circle of the first end face 21, that is, the agitator 51 has a large overlapping area with the first end face 21 in the radial direction of the first end face 21. During the rotation of the agitator 51, the surging insulating slurry can cover the inner circle and the outer circle of the first end face 21. The first end face 21 can be wetted with the insulating slurry once by rotating the agitator 51 one circle, and the wettability is high.

[0132] According to some embodiments of the present application, along the central axis P of the pole piece coil 2 , the projection of the agitator 51 extends from the outer circle to the inner circle of the first end surface 21 .

[0133] For example, the extension length of the agitator 51 is equal to the distance between the outer circle and the inner circle of the first end face 21, and, along the central axis P of the pole piece roll 2, on a plane perpendicular to the central axis P of the pole piece roll 2, the projection of the agitator 51 overlaps with the first end face 21.

[0134] In the above scheme, along the central axis P of the pole piece coil 2, there is a large overlapping area between the agitator 51 and the first end face 21. The waves 31 formed by the agitator 51 stirring the insulating slurry can cover the inner and outer circles of the first end face 21, so that the insulating slurry can infiltrate the inner and outer circles of the first end face 21, thereby improving the wetting efficiency.

[0135] Please refer to Figure 4 According to some embodiments of the present application, before the insulating slurry is stirred by rotating the stirring member 51, the stirring member 51 is located in the insulating slurry and the stirring member 51 does not exceed the liquid surface of the insulating slurry.

[0136] The stirring member 51 is located in the insulating slurry, so that the stirring member 51 drives the insulating slurry to ripple, so that the insulating slurry surges, thereby forming waves 31 .

[0137] The stirring member 51 does not exceed the liquid level of the insulating slurry. The stirring member 51 may be flush with the liquid level of the insulating slurry, or the stirring member 51 may be lower than the liquid level of the insulating slurry.

[0138] When the pole piece 11 is rolled up on the winding roller 20 to form the pole piece coil 2, one end of the winding roller 20 protrudes from the first end surface 21, so that the winding roller 20 has a better supporting effect on the pole piece 11. If the agitator 51 exceeds the liquid level of the insulating slurry, the agitator 51 is easy to interfere with the winding roller 20.

[0139] In the above solution, the agitator 51 does not exceed the liquid surface of the insulating slurry, which can reduce the risk of interference between the agitator 51 and the winding roller 20 of the winding sub-pole piece 11.

[0140] According to some embodiments of the present application, before the agitator 51 is rotated to stir the insulating slurry, the agitator 51 may also exceed the liquid surface of the insulating slurry. At this time, the agitator 51 needs to avoid the winding roller 20 of the winding sub-pole piece 11.

[0141] In the above embodiment, when the agitator 51 stirs the insulating slurry, the agitator 51 rotates parallel to the first end surface 21 , that is, the agitator 51 rotates along the circumference of the pole piece coil 2 so as to cover the insulating slurry on the entire area of ​​the first end surface 21 .

[0142] According to some embodiments of the present application, after the first end surface 21 of a pole piece coil 2 is wetted, the stirring speed of the insulating slurry is reduced, a pole piece coil 2 to be insulated is replaced, and the insulating slurry is repeatedly stirred.

[0143] After the first end face 21 of a pole piece coil 2 is soaked, the stirring speed of the insulating slurry is reduced to make the insulating slurry static and reduce the height of the insulating slurry surge, so as to facilitate the replacement of the pole piece coil 2 to be insulated and reduce the risk of the insulating slurry splashing to other areas when the pole piece coil 2 is replaced. After the pole piece coil 2 that is not soaked with the insulating slurry is replaced, the insulating slurry is repeatedly stirred to soak the first end face 21 of the insulating slurry, thereby improving the efficiency of the pole piece insulation treatment.

[0144] Please refer to Figure 6 , Figure 6 A schematic block diagram of the structure of a pole piece manufacturing device provided in some embodiments of the present application, Figure 7 A schematic diagram of the structure of a pole piece manufacturing device provided for some embodiments of the present application. According to some embodiments of the present application, the embodiments of the present application provide a pole piece manufacturing device, which can be used for the pole piece insulation processing method provided in any of the above embodiments. The pole piece manufacturing device includes a slitting device 100, a winding device 200, a container 300, a positioning device 400 and a stirring device 500. The slitting device 100 is used to slit the pole piece 1 into a plurality of sub-pole pieces 11; the winding device 200 is used to wind up the sub-pole piece 11 to form a pole piece coil 2, and the pole piece coil 2 includes a first end face 21 formed by the slitting edge of the sub-pole piece 11; the container 300 is used to contain the insulating slurry; the positioning device 400 is used to position the pole piece coil 2; the stirring device 500 is used to stir the insulating slurry in the container 300, so that the surging insulating slurry infiltrates the first end face 21, so as to form an insulating layer that at least covers the current collector of the sub-pole piece 11 and the burrs generated after the current collector is cut.

[0145] The slitting device 100 is a device for slitting a pole piece 1 into a plurality of sub-pole pieces 11, where the pole piece 1 may be a pole piece 1 raw material, and the sub-pole piece 11 may be a pole piece 1 constituting a battery cell. The slitting device 100 may include an upper cutter and a lower cutter, which are engaged with each other to cut the pole piece 1. The specific structure and working principle of the slitting device 100 may refer to the existing slitting device 100, and this application will not provide a detailed description.

[0146] The pole piece 1 is cut into a plurality of sub-pole pieces 11. After the sub-pole pieces 11 are wound to form the pole piece coil 2, the cut edge on one side of the sub-pole piece 11 constitutes a first end face 21. Along the extension direction of the central axis P of the pole piece coil 2, the first end face 21 as a whole can be regarded as an annular surface, and the first end face 21 has an inner circle and an outer circle, the inner circle is close to the central axis P of the pole piece coil 2, and the outer circle is far from the central axis P of the pole piece coil 2.

[0147] The winding device 200 is a device for winding the sub-pole sheet 11. The winding device 200 may include a winding drive and a winding roller 20, the winding roller 20 is connected to the winding drive, and the winding drive can drive the winding roller 20 to rotate, so as to wind the sub-pole sheet 11 on the winding roller 20. After the sub-pole sheet 11 is rolled up to form a pole sheet coil 2, when the pole sheet coil 2 moves between different processes, the winding roller 20 can move synchronously with the pole sheet coil 2.

[0148] One end of the container 300 is open for the electrode coil 2 to extend into.

[0149] The positioning device 400 is a device for positioning the pole piece coil 2 .

[0150] In some embodiments, please refer to Figure 7 The positioning device 400 may include a positioning fixture 41 and a fixing frame 42. The positioning fixture 41 is used to clamp the electrode coil 2. The fixing frame 42 may be connected to the container 300 or to other components (such as the foundation of a factory building) to facilitate the positioning of the electrode coil 2. In other embodiments, the positioning device 400 may also include a manipulator to achieve the positioning of the electrode coil 2. When the electrode coil 2 moves to the station where the insulating slurry is located, the relative position of the electrode coil 2 and the container 300 is adjusted by the positioning device 400. For example, the electrode coil 2 can be positioned outside the container 300 or inside the container 300.

[0151] The stirring device 500 is a device for stirring the insulating slurry. When the stirring device 500 is working, the insulating slurry in the container 300 can be rippled, so that the insulating slurry surges, and waves 31 are created in the container 300, so that the surged insulating slurry infiltrates the first end surface 21.

[0152] According to the pole piece manufacturing equipment of the embodiment of the present application, the pole piece 1 is cut into a plurality of sub-pole pieces 11 by the slitting device 100, the winding device 200 can wind up the sub-pole piece 11 to form a pole piece roll 2, and the positioning device 400 can realize the positioning of the pole piece roll 2, so that the insulating slurry stirred by the stirring device 500 can infiltrate the first end surface 21, and form an insulating layer on the first end surface 21 to cover the current collector and the burrs generated after the current collector is cut. The manufactured pole piece 1 can reduce the risk of burrs piercing the isolation membrane and causing internal short circuit of the battery cell, and can improve the reliability of the battery cell.

[0153] Please refer to Figure 7 According to some embodiments of the present application, the stirring device 500 includes a stirring member 51 and a driving member 52. The stirring member 51 is arranged in the insulating slurry. The driving member 52 is transmission-connected to the stirring member 51. The driving member 52 is used to drive the stirring member 51 to rotate relative to the container 300 to surge the insulating slurry.

[0154] The driving member 52 is a member for driving the stirring member 51 to rotate, and provides rotational power for the stirring member 51. The faster the driving member 52 drives the stirring member 51 to rotate, the higher the peak height of the waves 31 formed by the stirring member 51 stirring the insulating slurry is.

[0155] The stirring member 51 may be a plate-shaped structure. The stirring member 51 may be located in the insulating slurry and may not exceed the liquid surface of the insulating slurry.

[0156] In some embodiments, the stirring device 500 further includes a turntable 53, the stirring member 51 is connected to the turntable 53, and the turntable 53 is drivingly connected to the output end of the driving member 52. The driving member 52 can be a motor, and the output shaft of the motor can be connected to the turntable 53. The turntable 53 is driven by the motor to rotate, so as to drive the stirring member 51 to rotate relative to the container 300, thereby stirring the insulating slurry.

[0157] In some embodiments, the pole piece manufacturing equipment may further include a controller and a detection device 600, the controller is electrically connected to the driving member 52 and the detection device 600, the detection device 600 is used to detect the peak height of the waves 31 formed by the insulating slurry, and the controller is used to control the driving member 52 to adjust the rotation speed of the agitator 51 according to the peak height detected by the detection device 600.

[0158] The controller may be a PLC (Programmable Logic Controller); the detection device 600 may include, but is not limited to, a laser rangefinder and a CCD (Charge-coupled Device).

[0159] In the above scheme, the agitator 51 driven by the driving member 52 can cause the insulating slurry in the container 300 to surge, so that the surged insulating slurry infiltrates the first end surface 21, and then forms an insulating layer on the first end surface 21, with a simple structure and convenient operation.

[0160] According to some embodiments of the present application, the rotation axis of the agitator 51 is colinear with the central axis of the container 300 .

[0161] The rotation axis of the agitator 51 can be colinear with the central axis P of the pole piece coil 2 so that the insulation slurry that surges up when the agitator 51 rotates can cover the inner circle and the outer circle of the first end surface 21 .

[0162] The rotation axis of the agitator 51 is colinear with the central axis of the container 300 , so as to facilitate the positioning of the pole sheet roll 2 in the container 300 according to the rotation axis of the agitator 51 .

[0163] When the electrode sheet coil 2 is placed in the container 300 , the rotation axis of the agitator 51 may be colinear with the central axis P of the electrode sheet coil 2 , and the agitator 51 may be located on one side of the central axis P of the electrode sheet coil 2 .

[0164] According to some embodiments of the present application, the inner contour of the container 300 may be circular so as to match with the pole piece coil 2 .

[0165] According to some embodiments of the present application, an embodiment of the present application provides a method for insulating a pole piece, the method comprising:

[0166] like Figure 2 As shown, the pole piece 1 is cut into a plurality of sub-pole pieces 11;

[0167] Rolling up the sub-pole sheet 11 to form a pole sheet coil 2, wherein the pole sheet coil 2 includes a first end surface 21 formed by the cut edge of the sub-pole sheet 11;

[0168] like Figure 4 As shown, the pole piece coil 2 is placed in a container 300 containing insulating slurry, the first end surface 21 is arranged facing the insulating slurry, the first end surface 21 is parallel to the liquid surface of the insulating slurry, and the first end surface 21 does not contact the insulating slurry;

[0169] like Figure 5 and Figure 7 As shown, the insulating slurry is stirred by rotating the stirring member 51 so that the insulating slurry forms a wave 31, and the crest of the wave 31 is higher than the first end surface 21, so that the surging insulating slurry infiltrates the first end surface 21 to form an insulating layer that at least covers the current collector of the sub-pole sheet 11 and the burrs generated after the current collector is cut.

[0170] Among them, the rotation axis of the agitator 51 is colinear with the central axis of the pole piece coil 2; the extension direction of the agitator 51 passes through the central axis P of the pole piece coil 2; the agitator 51 is located on one side of the central axis P of the pole piece coil 2, and the two ends of the agitator 51 along the extension direction of the agitator 51 exceed the inner circle and outer circle of the first end face 21.

[0171] The pole piece 1 manufactured according to the technical solution of the present application can form an insulating layer at the cutting edge, and the insulating layer can cover the burrs. When manufactured into a battery cell, the risk of the burrs piercing the isolation membrane and causing an internal short circuit in the battery cell can be reduced, so that the battery cell can have higher reliability.

[0172] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for insulating a pole piece, It is characterized in that include: Cutting the pole piece into a plurality of sub-pole pieces; Rolling up the sub-pole sheet to form a pole sheet coil, wherein the pole sheet coil includes a first end surface formed by the cut edge of the sub-pole sheet; Arrange the first end surface facing the insulating slurry; The insulating slurry is infiltrated into the first end surface to form an insulating layer that at least covers the current collector of the sub-electrode sheet and burrs generated after the current collector is cut.

2. The electrode insulation treatment method according to claim 1, It is characterized in that The step of soaking the first end surface with the insulating slurry comprises: The insulating slurry is stirred so that the surging insulating slurry infiltrates the first end surface.

3. The electrode insulation treatment method according to claim 2, It is characterized in that Before the insulating slurry is stirred, the first end surface is not in contact with the insulating slurry.

4. The electrode insulation treatment method according to claim 3, It is characterized in that The stirring of the insulating slurry comprises: The insulating slurry is stirred so that the insulating slurry forms waves, and the crest of the wave is higher than the first end surface.

5. The pole piece insulation treatment method according to claim 4, It is characterized in that Before the insulating slurry is stirred, the distance between the first end surface and the insulating slurry is H 1 , after the insulating slurry is stirred to form the wave, the wave crest height is H 2 , meet, 1mm≤H 2 -H 1 ≤5mm.

6. The electrode insulation treatment method according to claim 5, It is characterized in that 2mm≤H 2 -H 1 ≤4mm。 7. The pole piece insulation processing method according to claim 2, It is characterized in that When the insulating slurry is stirred, the pole piece coil does not rotate.

8. The electrode insulation processing method according to claim 2, It is characterized in that The stirring of the insulating slurry comprises: The insulating slurry is stirred by rotating a stirring member, and the rotation axis of the stirring member is colinear with the central axis of the pole piece coil.

9. The pole piece insulation processing method according to claim 8, It is characterized in that The extension direction of the stirring member intersects with the central axis of the pole piece coil.

10. The pole piece insulation processing method according to claim 9, It is characterized in that Along the extension direction of the central axis of the pole piece coil, the projection of the stirring member is located on one side of the central axis of the pole piece coil.

11. The electrode insulation treatment method according to claim 9 or 10, It is characterized in that Along the extension direction of the central axis of the pole piece coil, two ends of the projection of the agitator along the extension direction of the agitator exceed the inner circle and the outer circle of the first end surface.

12. The pole piece insulation processing method according to claim 8, It is characterized in that Before the insulating slurry is stirred by rotating the stirring member, the stirring member is located in the insulating slurry and the stirring member does not exceed the liquid level of the insulating slurry.

13. The pole piece insulation processing method according to claim 2, It is characterized in that After the first end surface of one of the pole piece coils is wetted, the stirring speed of the insulating slurry is reduced, and a pole piece coil to be insulated is replaced, and the stirring of the insulating slurry is repeated.

14. A pole piece manufacturing device, It is characterized in that include: A slitting device, used for slitting a pole piece into a plurality of sub-pole pieces; A winding device, used for winding the sub-pole sheet to form a pole sheet coil, wherein the pole sheet coil includes a first end surface formed by the cut edge of the sub-pole sheet; A container for containing insulating slurry; A positioning device, used for positioning the pole piece coil; A stirring device is used to stir the insulating slurry in the container so that the surging insulating slurry infiltrates the first end surface to form an insulating layer that at least covers the current collector of the sub-electrode sheet and burrs generated after the current collector is cut.

15. The pole piece manufacturing equipment according to claim 14, It is characterized in that The stirring device comprises a stirring member and a driving member, wherein the stirring member is arranged in the insulating slurry, the driving member is transmission-connected with the stirring member, and the driving member is used for driving the stirring member to rotate relative to the container to surge the insulating slurry.

16. The pole piece manufacturing equipment according to claim 15, It is characterized in that The rotation axis of the agitator is colinear with the central axis of the container.

Citation Information

Patent Citations

  • Lithium ion rechargeable electrochemical cell with insulating tab and method of forming same

    CN115332735A

  • Battery cell pole piece manufacturing method, battery cell manufacturing method, battery cell and battery

    CN115911277A

  • Flooding coating device

    CN206661574U

  • Positive pole piece and battery

    CN216750238U

  • Nonaqueous electrolytic secondary battery and the manufacturing method thereof