Graphene (at) C (at) lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

By electronegative treatment of graphene oxide and electrostatic combination with chitosan, the problem of electrochemical inert component activation reaction of lithium-rich manganese-based positive electrode material during the first charge and insufficient graphene coating effect was solved, and the problem of the lithium-rich manganese-based positive electrode material was solved. The uniform and dense coating of graphene@C@lithium-rich manganese-based positive electrode material improves the electrochemical performance and stability of the material.

CN119069674AInactive Publication Date: 2024-12-03YANCHENG TEACHERS UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411205637.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The electrochemical inert component activation reaction of existing lithium-rich manganese-based positive electrode materials during the first charge leads to a decrease in Coulomb efficiency and insufficient graphene coating effect, resulting in no significant improvement in the material's conductivity.

Method used

The graphene oxide after electronegative treatment is complexed with lithium, nickel and manganese sources, and electrostatically bound with electropositive chitosan. The dispersion and binding of graphene are improved through double-coating method. The ability to form a uniform and dense graphene @C@lithium-rich manganese-based positive electrode material.

Benefits of technology

Improve the electrochemical performance of the material, enhance the rate performance and stability, achieve uniform and dense coating of graphene and amorphous carbon, improve the coating effect of Li1.2Mn0.6Ni0.2O2, and improve the structural density of the material. and electrochemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069674A_ABST
    Figure CN119069674A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of positive electrode materials, and particularly relates to a graphene (at) C (at) lithium-rich manganese-based positive electrode material and a preparation method and application of the graphene (at) C (at) lithium-rich manganese-based positive electrode material. And the graphene oxide with electronegativity and the chitosan with electropositivity are subjected to electrostatic binding, so that the dispersity of the graphene in the chitosan is improved, the binding capacity of the graphene oxide with a lithium source, a nickel source and a manganese source is improved, and the lithium-rich manganese-based positive electrode material uniformly and compactly coated with the graphene and amorphous carbon is obtained. The composite material is used as an electrode material to be applied to preparation of a lithium ion battery positive pole piece.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of positive electrode materials, and specifically relates to graphene@C@lithium-rich manganese-based positive electrode materials and preparation methods and applications thereof. Background Art

[0002] Lithium-ion batteries are considered to be ideal energy storage and conversion devices due to their high energy density, high specific capacity, no memory effect and environmental friendliness. At present, due to the popularity of electric vehicles, portable electronic devices and smart grids, the demand for the energy density and cycle life of lithium-ion batteries continues to increase, and the selection and application of positive electrode materials have a profound impact on the performance, service life and cost of lithium-ion batteries. At present, the discharge specific capacity of commercial lithium battery positive electrode materials such as LiCoO2, LiMn2O4, and LiFePO4 is much lower than that of negative electrode materials, which restricts the further improvement of lithium-ion battery performance. Therefore, new positive electrode materials have developed rapidly in recent years, among which lithium-rich manganese-based positive electrode materials have been widely studied due to their high discharge specific capacity.

[0003] The structural formula of lithium-rich manganese-based positive electrode materials is xLi2MnO3·(1-x)LiMO2 (M = Ni, Mn, Co, etc.), which is believed to be composed of a monoclinic layered lithium-rich phase Li2MnO3 and a hexagonal layered LiNi 0.5 Mn 0.5 O2 composition, both have α-NaFeO2 structure. Among the lithium-rich manganese-based positive electrode material systems, the most researched is Li 1.2 Mn 0.6 Ni 0.2 O2 material, its specific capacity at 0.1C rate can reach 300mAh / g, but when the material is charged to about 4.5V for the first time, the electrochemically inert component Li2MnO3 undergoes activation reaction, Li + Escape, accompanied by O 2- MnO2 is generated by oxidation reaction, and LiMnO2 is formed after discharge and lithium insertion, resulting in the problem of reduced initial coulombic efficiency.

[0004] In order to overcome this shortcoming, people have made a lot of attempts. It has been confirmed that carbon coating is a simple and effective method to enhance the first coulombic efficiency, rate performance and stability. It can greatly improve the rate performance of positive electrode materials by increasing the electron transfer rate of the material. Considering that the unique structure of graphene gives it many unique properties, such as high specific surface area (theoretically 2630m 2 .g -1), outstanding electronic conductivity and excellent mechanical properties, but because graphene is a two-dimensional material, it often cannot wrap the lithium-rich manganese-based positive electrode material well to form an ideal core-shell structure, which ultimately leads to the overall conductivity of the material not being significantly improved. In order to overcome this technical defect, a large amount of graphene still needs to be added, but the result is still unsatisfactory. On this basis, after further research, it was found that the method of double coating with graphene and amorphous carbon can effectively make up for the problem of insufficient graphene coating effect.

[0005] The uniformity of the carbon layer and the density of the conductive network have an important influence on the electrochemical performance of the product. Although the current double-coating method has solved the problem of poor graphene coating to a certain extent, the carbon source and graphene are often directly blended in order to achieve the purpose of uniform dispersion of the carbon source and graphene through longer blending time and more sophisticated blending operations, and the lithium-rich manganese-based positive electrode material is coated with the carbon source and graphene together. However, blending inevitably fails to make the carbon source and graphene completely evenly dispersed, so that after calcination, the problems of structural heterogeneity, non-density, and incomplete coating still exist. Summary of the invention

[0006] In view of the deficiencies in the above-mentioned prior art, the present invention provides a graphene@C@lithium-rich manganese-based positive electrode material and a preparation method and application thereof. After the graphene oxide is subjected to electronegativity treatment, the electronegative graphene oxide is used to complex a lithium source, a nickel source and a manganese source, and the electronegative graphene oxide is used to electrostatically combine with electropositive chitosan, thereby increasing and improving the dispersibility of graphene in chitosan, and at the same time improving the binding ability of graphene oxide with the lithium source, nickel source, manganese source and chitosan, so as to obtain a lithium-rich manganese-based positive electrode material uniformly and densely coated with graphene and amorphous carbon.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0008] The preparation method of graphene@C@ lithium-rich manganese-based positive electrode material comprises the following steps:

[0009] Lithium source, nickel source and manganese source were weighed according to the molar ratio of Li:Ni:Mn of 1.2:0.2:0.6, and then dissolved in anhydrous ethanol to obtain raw materials. Lithium source, nickel source and manganese source were used together to prepare Li 1.2 Mn 0.6 Ni 0.2 O2;

[0010] The graphene oxide is dispersed by anhydrous ethanol, and then the graphene oxide is subjected to electronegativity modification treatment by using a modifier triethylamine. The graphene oxide surface contains a large number of carboxyl groups. When the graphene oxide is subjected to the modification treatment by using triethylamine, the triethylamine is used to drive away hydrogen on the carboxyl groups of the graphene oxide, so that the graphene oxide is electronegative. The electronegative graphene oxide is convenient for complexing with metal cations of lithium source, nickel source and manganese source, and is also convenient for electrostatically combining with electropositive chitosan, thereby improving the dispersibility of graphene in chitosan and enhancing the interface binding force between the graphene oxide and chitosan. The modifier triethylamine is then removed by washing with a large amount of anhydrous ethanol to obtain the treated graphene oxide.

[0011] The raw material and the treated graphene oxide are mixed to obtain a mixture, and during the mixing process, the electronegative graphene oxide is complexed with metal cations of the lithium source, the nickel source and the manganese source. The mixture is blended with chitosan and then ground to obtain a precursor. During the grinding process, the electronegative graphene oxide and the electropositive chitosan are electrostatically bonded, thereby improving the coating and dispersion effects;

[0012] The precursor is calcined to obtain graphene@C@ lithium-rich manganese-based positive electrode material. The calcination process realizes Li 1.2 Mn 0.6 Ni 0.2 Preparation of O2, reduction of graphene oxide and carbonization of chitosan to directly obtain graphene@C@lithium-rich manganese-based positive electrode materials.

[0013] Preferably, the modifier is triethylamine, the amount of the modifier is excessive, and the modification method is: blending graphene oxide, triethylamine and anhydrous ethanol, ultrasonicating at room temperature for 0.5-1h, and then magnetically stirring for 3-5h.

[0014] Preferably, the mass ratio of the raw material to the treated graphene oxide is 100:2-4. Since the treated graphene oxide in the present invention can be evenly dispersed and can be complexed with metal ions, the electrochemical performance can be excellently improved without adding a large amount.

[0015] Preferably, the mass ratio of chitosan to treated graphene oxide is 10-20:1. Carbon does not participate in the electrochemical reaction in the positive electrode material. Too much carbon coating will reduce the content of active substances, resulting in a decrease in the specific capacity of the material. However, too low carbon content will not significantly improve the electrochemical performance of the material and reduce the coating.

[0016] Preferably, the calcination conditions are: in an inert atmosphere, first carbonize at 300-400° C. for 2-3 h, and then calcine at 700-900° C. for 16-20 h.

[0017] Preferably, natural graphite is prepared by Hummer ,s reaction for oxidation to obtain graphene oxide. Natural graphite is cheap.

[0018] Preferably, during the blending process of the mixture and chitosan, acetic acid with a volume fraction of 5% is also added as a solvent. The acetic acid can dissolve the chitosan, thereby enhancing the electrostatic bonding ability between the chitosan and the treated graphene oxide.

[0019] The present invention also protects the graphene@C@lithium-rich manganese-based positive electrode material prepared by the above preparation method, wherein the graphene@C@lithium-rich manganese-based positive electrode material is Li 1.2 Mn 0.6 Ni 0.2 O2, using graphene and C to Li 1.2 Mn 0.6 Ni 0.2 O2 is double-carbon coated.

[0020] The present invention also protects the application of graphene@C@lithium-rich manganese-based positive electrode material in the preparation of positive electrode sheets of lithium-ion batteries.

[0021] Preferably, the positive electrode sheet of a lithium-ion battery is prepared according to the following steps:

[0022] The graphene@C@ lithium-rich manganese-based positive electrode material, the conductive agent and the binder are added to N-methylpyrrolidone, mixed and ground to obtain a slurry, and the slurry is evenly coated on the current collector aluminum foil, and dried and pressed to prepare a positive electrode sheet for a lithium-ion battery;

[0023] The binder is selected from one or more of polyvinylidene fluoride, polyacrylic acid, sodium carboxymethyl cellulose, sodium alginate, and gelatin, and the conductive agent is selected from carbon nanotubes, carbon black, Super-P, or Ketjen black;

[0024] The mass ratio of graphene@C@lithium-rich manganese-based positive electrode material, conductive agent and binder is 8:1:1.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. Chitosan is obtained by deacetylation of chitin and is a natural biopolysaccharide polymer material with wide application value. The present invention uses chitosan as raw material and chitosan as the main carbon source. Chitosan has a C2NH2 structure and is easily protonated into -NH3 + , so that chitosan is positively charged; in addition, chitosan can form different types of network structures under different intramolecular or intermolecular interactions, thereby improving the coating of lithium, nickel and manganese sources. The chitosan in chitosan mainly comes from the shells of shrimps and crabs. Its utilization allows biological resources to be fully recycled, can achieve better economic benefits, and reduce environmental pollution.

[0027] 2. Considering the technical defects of the double carbon coating in the prior art, the present invention treats the graphene oxide for electronegativity and screens the carbon source, so that in the obtained precursor, the reduced graphene oxide is the center, and chitosan and the lithium source, nickel source and manganese source are stably complexed on the reduced graphene oxide, thereby making the precursor have the characteristics of structural stability. Therefore, after calcination, the obtained graphene@C@lithium-rich manganese-based positive electrode material can achieve the graphene and amorphous carbon to Li 1.2 Mn 0.6 Ni 0.2 O2 is evenly coated and has a dense structure.

[0028] 3. The present invention uses graphene oxide, lithium source, nickel source, manganese source and chitosan as raw materials, and after a step of high temperature calcination, Li 1.2 Mn 0.6 Ni 0.2 The preparation of O2, reduction of graphene oxide and carbonization of chitosan were carried out, and graphene@C@lithium-rich manganese-based positive electrode materials were obtained, which is easy to operate.

[0029] 4. Graphene is different from ordinary carbon materials in its 3D structure, which provides an embedding / ejection channel for lithium ions. However, the two-dimensional layered structure of graphene is prone to self-agglomeration, resulting in capacity decay. Based on this, the present invention uses graphene oxide as a raw material. Graphene oxide can achieve excellent dispersion, thereby improving the combination with lithium source, nickel source, manganese source, and chitosan in the precursor, improving the dispersibility, and at the same time improving the Li 1.2 Mn 0.6 Ni 0.2 The coating effect of O2. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 In the figure, (a) and (b) are scanning electron microscope images of the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1 at different magnifications, (c) is a transmission electron microscope image of the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1, and (d) is a transmission electron microscope image of the graphene @ C @ lithium-rich manganese-based positive electrode material of Comparative Example 1;

[0031] Figure 2 The electrochemical impedance diagram of the graphene@C@lithium-rich manganese-based positive electrode material of Example 1 and the graphene@C@lithium-rich manganese-based positive electrode material of Comparative Example 1;

[0032] Figure 3 The graph is a cycle performance diagram of the graphene@C@lithium-rich manganese-based positive electrode material of Example 1 at different rates;

[0033] Figure 4 This is a charge and discharge curve diagram of the graphene@C@lithium-rich manganese-based positive electrode material of Example 1;

[0034] Figure 5 This is the cycle performance diagram of the graphene@C@lithium-rich manganese-based positive electrode material of Example 1. DETAILED DESCRIPTION

[0035] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.

[0036] The graphene oxide of the present invention is prepared according to the following steps:

[0037] Add 2g graphite powder, 5g NaNO3 and 46mL concentrated sulfuric acid to a 500mL three-necked flask, put it in an ice-water bath to keep the temperature below 5℃, and stir vigorously for 30min. Then, slowly add 6g KMnO4 and stir at 15℃ for 2h. After raising the reaction temperature to 35℃ and stirring for 30min, add 92mL deionized water dropwise to the viscous mixture, and then transfer the three-necked flask to a 98℃ oil bath and continue stirring for 15min. Add 6mL 30% H2O2 and stir for 30min, then add 56mL deionized water to dilute. After standing and stratifying, the above mixture is transferred to a dialysis bag and placed in deionized water. The deionized water is continuously replaced until the pH value reaches neutral.

[0038] The technical solution of the present invention is further studied by using embodiments and comparative examples below. The specific research methods and results are as follows:

[0039] Example 1

[0040] A method for preparing a graphene@C@ lithium-rich manganese-based positive electrode material comprises the following steps:

[0041] S1. LiNO3, Ni(CH3COO)2·4H2O and Mn(CH3COO)2·4H2O are weighed in a Li:Ni:Mn molar ratio of 1.2:0.2:0.6, and then dissolved in anhydrous ethanol to obtain a raw material;

[0042] S2, dispersing 30 mg of graphene oxide in anhydrous ethanol, and then using 240 μL of a modifier triethylamine for electronegativity modification, first ultrasonicating at room temperature for 1 hour, then magnetically stirring for 3 hours, and then using a large amount of anhydrous ethanol to wash away the triethylamine to obtain treated graphene oxide;

[0043] S3, after mixing the raw material and the treated graphene oxide, ultrasonically treat for 15 minutes and let stand for 1 hour to obtain a mixture; wherein the mass ratio of the total amount of the lithium source, the nickel source and the manganese source to the treated graphene oxide is 100:3;

[0044] S4, mixing the mixture, chitosan and 5% by volume acetic acid solution and grinding them to obtain a precursor;

[0045] Among them, the mass ratio of chitosan to treated graphene oxide is 15:1;

[0046] S5. The precursor is first carbonized at 350°C for 2.5h, and then calcined at 800°C for 18h to obtain graphene@C@lithium-rich manganese-based positive electrode material.

[0047] Example 2

[0048] A method for preparing a graphene@C@ lithium-rich manganese-based positive electrode material comprises the following steps:

[0049] S1. LiNO3, Ni(CH3COO)2·4H2O and Mn(CH3COO)2·4H2O are weighed in a Li:Ni:Mn molar ratio of 1.2:0.2:0.6, and then dissolved in anhydrous ethanol to obtain a raw material;

[0050] S2, dispersing 30 mg of graphene oxide in anhydrous ethanol, and then using 240 μL of a modifier triethylamine for electronegativity modification, first ultrasonicating at room temperature for 0.5 h, then magnetically stirring for 4 h, and then using a large amount of anhydrous ethanol to wash away the triethylamine to obtain treated graphene oxide;

[0051] S3, mixing the raw material and the treated graphene oxide, ultrasonicating for 15 minutes and standing for 1 hour to obtain a mixture;

[0052] The mass ratio of the total amount of lithium source, nickel source and manganese source to the processed graphene oxide is 100:2;

[0053] S4, mixing the mixture, chitosan and 5% by volume acetic acid solution and grinding them to obtain a precursor;

[0054] Among them, the mass ratio of chitosan to treated graphene oxide is 10:1;

[0055] S5. The precursor is first carbonized at 300°C for 3 hours, and then calcined at 900°C for 16 hours to obtain graphene@C@lithium-rich manganese-based positive electrode material.

[0056] Example 3

[0057] A method for preparing a graphene@C@ lithium-rich manganese-based positive electrode material comprises the following steps:

[0058] S1. LiNO3, Ni(CH3COO)2·4H2O and Mn(CH3COO)2·4H2O are weighed in a Li:Ni:Mn molar ratio of 1.2:0.2:0.6, and then dissolved in anhydrous ethanol to obtain a raw material;

[0059] S2, dispersing 30 mg of graphene oxide in anhydrous ethanol, and then using 240 μL of a modifier triethylamine for electronegativity modification, first ultrasonicating at room temperature for 1 h, then magnetically stirring for 2 h, and then using a large amount of anhydrous ethanol to wash away the triethylamine to obtain treated graphene oxide;

[0060] S3, mixing the raw material and the treated graphene oxide, ultrasonicating for 15 minutes and standing for 1 hour to obtain a mixture;

[0061] The mass ratio of the total amount of lithium source, nickel source and manganese source to the processed graphene oxide is 100:4;

[0062] S4, mixing the mixture, chitosan and 5% by volume acetic acid solution and grinding them to obtain a precursor;

[0063] Among them, the mass ratio of chitosan to treated graphene oxide is 20:1;

[0064] S5. The precursor is first carbonized at 400°C for 2h, and then calcined at 700°C for 20h to obtain graphene@C@lithium-rich manganese-based positive electrode material.

[0065] Comparative Example 1

[0066] A method for preparing a graphene@C@lithium-rich manganese-based positive electrode material, which has the same preparation steps as those in Example 1, except that chitosan is replaced with an equal amount of glucose, specifically comprising the following steps:

[0067] S1. LiNO3, Ni(CH3COO)2·4H2O and Mn(CH3COO)2·4H2O are weighed in a Li:Ni:Mn molar ratio of 1.2:0.2:0.6, and then dissolved in anhydrous ethanol to obtain a raw material;

[0068] S2, dispersing 30 mg of graphene oxide in anhydrous ethanol, and then using 240 μL of a modifier triethylamine for electronegativity modification, first ultrasonicating at room temperature for 1 hour, then magnetically stirring for 3 hours, and then using a large amount of anhydrous ethanol to wash away the triethylamine to obtain treated graphene oxide;

[0069] S3, mixing the raw material and the treated graphene oxide, ultrasonicating for 15 minutes and standing for 1 hour to obtain a mixture;

[0070] The mass ratio of the total amount of lithium source, nickel source and manganese source to the processed graphene oxide is 100:3;

[0071] S4, mixing the mixture, glucose and deionized water and grinding them to obtain a precursor;

[0072] Among them, the mass ratio of glucose to treated graphene oxide is 15:1;

[0073] S5. The precursor is first carbonized at 350°C for 2.5h, and then calcined at 800°C for 18h to obtain graphene@C@lithium-rich manganese-based positive electrode material.

[0074] In Examples 1-3 of the present invention, graphene and amorphous carbon are uniformly coated and the structure of the graphene@C@lithium-rich manganese-based positive electrode material is dense. The graphene@C@lithium-rich manganese-based positive electrode material of Example 1 is used as an example for research, and compared with the sample of Comparative Example 1. The specific research method and results are as follows:

[0075] Figure 1 The results show that the graphene@C@lithium-rich manganese-based cathode material of Example 1 has a spherical shape. In addition, the graphene@C@lithium-rich manganese-based cathode material samples of Example 1 and Comparative Example 1 were tested by transmission electron microscopy. The results show that although the Li 1.2 Mn 0.6 Ni 0.2 The morphology of O2 material tends to be spherical, but the size is large, and the contact between C and graphene is loose; while Li coated with chitosan and graphene 1.2 Mn 0.6 Ni 0.2 The O2 material is spherical in shape and small in size, and C is stably combined with graphene to form a composite material with a stable structure.

[0076] The following is a battery assembled using the graphene@C@lithium-rich manganese-based positive electrode materials of Example 1 of the present invention and Comparative Example 1. The battery assembly method is as follows:

[0077] Weigh 0.0375g of the binder polyvinylidene fluoride, and use a dropper to take 1g of N-methylpyrrolidone into a small beaker, add a small magnet, seal the cup mouth with plastic wrap, and stir magnetically for 30 minutes until it is completely dissolved, then add 0.0375g of the conductive agent and 0.5g of the graphene@C@ lithium-rich manganese-based positive electrode material, continue to seal the mouth and stir on a magnetic stirrer for 1.5h to fully mix, to obtain a viscous slurry, evenly apply the slurry on the current collector aluminum foil, and then dry it to obtain a positive electrode sheet;

[0078] Place the positive electrode in a vacuum drying oven at 70°C and dry it under vacuum. During the drying process, draw air 2-3 times to ensure that the vacuum is maintained in the vacuum drying oven so that the electrode can be fully dried. Take out the electrode and lay it on the positive electrode shell, absorb the electrolyte to soak the electrode, put in the diaphragm, soak it with electrolyte again, install the lithium sheet, wipe the battery clean with filter paper, and put it into the battery shell for blue electricity test.

[0079] Put the prepared battery shell into the test system, set the voltage to 4.8V at room temperature, and use the battery test system to test the charge and discharge performance under constant current conditions. The charge and discharge rates are 0.2C, 3C, 5C, 7C and 10C respectively. Set the number of cycles to 800 at room temperature, observe the change trend of the discharge specific capacity after 800 cycles, and test the cycle stability. To test the rate performance, set the charge and discharge rates to 0.2C, 3C, 5C, 7C and 10C respectively, and record the test data.

[0080] The battery is tested for AC impedance at a frequency of 10mHz to 100kHz. Figure 2 The EIS curves of the sample in Example 1 and the sample in Comparative Example 1 are given in the figure. The characterization results show that both of them form two semicircles in the high-frequency and medium-frequency regions, and form a slope line in the low-frequency region. Figure 2 It can be seen that the two semicircle diameters of the graphene @C@ lithium-rich manganese-based positive electrode material of Example 1 are relatively small in the high-frequency and medium-frequency bands, and it can be clearly seen that the graphene @C@ lithium-rich manganese-based positive electrode material of Example 1 has a higher slope in the low-frequency region, proving that the impedance value of the graphene @C@ lithium-rich manganese-based positive electrode material of Example 1 is relatively small. This is because the graphene @C@ lithium-rich manganese-based positive electrode material of Example 1 has high structural density and good uniformity, and the graphene and carbon completely cover the lithium-rich manganese-based positive electrode material, thereby providing Li + It provides a good migration environment. The graphene@C@ lithium-rich manganese-based cathode material of Example 1 has a small charge transfer impedance. + It has better kinetic performance. Therefore, the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1 has more excellent performance than the material of Comparative Example 1. The following only takes the graphene @ C @ lithium-rich manganese-based positive electrode material prepared in Example 1 as an example to test its electrochemical performance.

[0081] Figure 3This is the cycle performance diagram of the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1 at different rates. The discharge capacity at 0.2C rate when the number of cycles is 5 is 286.2 mAh / g, the discharge capacity at 3C rate when the number of cycles is 5 is 281.6 mAh / g, the discharge capacity at 5C rate when the number of cycles is 5 is 269.2 mAh / g, the discharge capacity at 7C rate when the number of cycles is 5 is 253.2 mAh / g, and the discharge capacity at 10C rate when the number of cycles is 5 is 232.3 mAh / g. It can be seen that the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1 has an excellent specific capacity. The second charge and discharge specific capacity at 0.2C is almost the same as the result of the first charge and discharge specific capacity at 0.2C. It can be seen that the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1 has a stable structure and excellent reversible performance.

[0082] Figure 4 This is the charge and discharge diagram of the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1. As can be seen from the figure, the charge and discharge platform of the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1 is stable at about 3.5V, and the discharge specific capacity is about 285mAh / g. It can be seen that the graphene @ C @ lithium-rich manganese-based positive electrode material of Example 1 has an excellent specific capacity.

[0083] Figure 5 The results show that the graphene@C@lithium-rich manganese-based cathode material of Example 1 has a specific capacity of 286.4 mAh / g in the first charge and discharge, and a specific capacity of 273.7 mAh / g after 800 charge and discharge cycles, with a retention rate of 95.6%. By analyzing the trend, it can be seen that the prepared graphene@C@lithium-rich manganese-based cathode material has a high specific capacity. Although it has a tendency to gradually decay during the cycle, it is generally stable in the cycle and maintains a very high specific capacity.

[0084] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalent technologies, the present invention is also intended to include these changes and variations. The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and their protection scope is not limited thereto. Equivalent substitutions or changes made by those skilled in the art on the basis of the present invention are all within the protection scope of the present invention, and the protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a graphene@C@ lithium-rich manganese-based positive electrode material, characterized in that: The steps include: A lithium source, a nickel source and a manganese source are weighed according to a molar ratio of Li:Ni:Mn of 1.2:0.2:0.6, and then dissolved in anhydrous ethanol to obtain a raw material; The graphene oxide is dispersed in anhydrous ethanol, and then a modifier is used to perform electronegativity modification, and then the modifier is removed to obtain treated graphene oxide; The raw material and the treated graphene oxide are mixed to obtain a mixture, and the mixture is blended with chitosan and then ground to obtain a precursor; The precursor is calcined in the absence of oxygen to obtain graphene@C@lithium-rich manganese-based positive electrode material.

2. The method for preparing the graphene@C@lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The modifier is triethylamine.

3. The method for preparing the graphene@C@lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The mass ratio of the total amount of lithium source, nickel source and manganese source to the processed graphene oxide is 100:2-4.

4. The method for preparing the graphene@C@lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The mass ratio of chitosan to treated graphene oxide is 10-20:

1.

5. The method for preparing the graphene@C@lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The calcination conditions are: in an inert atmosphere, first carbonize at 300-400°C for 2-3h, and then calcine at 700-900°C for 16-20h.

6. A method for preparing the graphene@C@lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: Natural graphite is used in Hummer , s reaction is oxidized to obtain graphene oxide.

7. The method for preparing the graphene@C@lithium-rich manganese-based positive electrode material according to claim 6, characterized in that: During the blending process of the mixture and chitosan, acetic acid with a volume fraction of 5% is added as a solvent.

8. A graphene@C@lithium-rich manganese-based positive electrode material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: Li-rich manganese-based cathode material is Li 1.2 Mn 0.6 Ni 0.2 O2.

9. Use of the graphene@C@lithium-rich manganese-based positive electrode material according to claim 8 in the preparation of a positive electrode sheet for a lithium-ion battery.

10. The use according to claim 9, characterized in that: The positive electrode of the lithium-ion battery is prepared according to the following steps: Graphene@C@lithium-rich manganese-based positive electrode material, conductive agent and binder are added to N-methylpyrrolidone, mixed and ground to obtain slurry, and the slurry is evenly coated on the current collector. After drying and pressing, the positive electrode sheet of the lithium-ion battery is made.