Preparation method and application of multilayer composite solid electrolyte membrane

The preparation of high-valent metal atom doped rare earth metal oxide inorganic filler and multi-layer composite solid electrolyte membrane through electrospinning technology has solved the problems of low ionic conductivity and mechanical strength of solid electrolytes in lithium metal batteries and improved the energy density of the battery and cycle stability reduce safety risks.

CN119069818AActive Publication Date: 2024-12-03EAST CHINA UNIV OF SCI & TECH

Patent Information

Application Number
CN202411226235.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-11
Filing Date
2024-09-03
Publication Date
2024-12-03
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Existing lithium metal batteries have safety hazards due to the use of flammable and unstable organic electrolytes, such as thermal runaway, the risk of battery fire or explosion. At the same time, the room temperature ionic conductivity of solid electrolytes is low, mechanical strength is poor, and thermal. Poor stability limits its application.

Method used

Electrospinning and high-temperature heat treatment technology are used to prepare high-valent metal atom-doped rare earth metal oxide inorganic fillers with oxygen-rich vacancies. Combining lithium salts and polymer matrix, multi-layer composite solid electrolyte nanofiber membranes are prepared by electrospinning to form "Sandwich" structure enhances the ion transport channel and mechanical strength of the electrolyte.

Benefits of technology

It significantly improves the transmission rate of lithium ions and the mechanical strength of the electrolyte, broadens the electrochemical window, improves the energy density and cycle stability of lithium batteries, extends the cycle life of the battery, and reduces safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069818A_ABST
    Figure CN119069818A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a multilayer composite solid electrolyte membrane. The preparation method comprises the following steps: preparing oxygen vacancy-rich high-valence metal atom doped rare earth metal oxide as an inorganic filler of the composite solid electrolyte by adopting an electrostatic spinning and high-temperature heat treatment technology; and then dispersing the nano-fiber, a lithium salt and a polymer matrix into a solvent to obtain different electrostatic spinning precursor solutions, and spinning multiple layers of composite solid electrolyte nano-fiber membranes on a receiver in sequence. The prepared multi-layer composite solid electrolyte nanofiber membrane has good compatibility with lithium metal and can be used in cooperation with a high-voltage positive electrode material, the energy density of a lithium battery is improved, an electrochemical window is widened, and meanwhile the problems that the size, the weight and the total resistance of the battery are increased and the like can be effectively solved through the ultrathin interface modification layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new energy battery materials and relates to a solid electrolyte for lithium batteries, and specifically relates to a multilayer composite solid electrolyte membrane and a preparation method thereof and an application thereof in the preparation of solid-state lithium batteries. Background Art

[0002] Since lithium metal has a high theoretical specific capacity (3860 mAh g -1 ) and low potential (-3.04V), lithium metal batteries are considered to be a promising technology in the future fields of smart grids, electric vehicles, etc. However, commercial lithium metal batteries have a series of safety issues due to the use of flammable and electrochemically unstable organic electrolytes. For example, the electrolyte is very likely to cause thermal runaway during battery use, especially in overcharge or short circuit conditions, which may cause the battery to catch fire or explode.

[0003] At present, the development of solid electrolytes with no liquid flow, non-flammable and non-explosive properties, good flexibility and strong processability is considered to be the best solution to eliminate the safety hazards of organic liquid electrolytes. At the same time, solid electrolytes can effectively inhibit the growth of lithium dendrites, thereby avoiding the side reactions caused by the growth of lithium dendrites piercing the diaphragm. However, solid electrolytes are limited in their application in lithium metal batteries due to their low room temperature ionic conductivity, poor mechanical strength, poor thermal stability, poor contact with the positive and negative electrode interfaces and poor compatibility. In response to this series of problems, researchers have proposed solutions from different angles, such as adding plasticizers, nanofillers, block copolymers, etc. to polymer electrolytes. However, the above methods have failed to meet the characteristics of ideal high-performance all-solid-state electrolytes. A single polymer structure usually does not have a wide enough energy band gap to withstand the reduction of the lithium metal negative electrode and the oxidation of the high-voltage positive electrode at the same time. Designing a multilayer composite electrolyte is an effective strategy to solve this problem. Summary of the invention

[0004] The present invention aims at the deficiencies of the prior art and provides a method for preparing and applying a multilayer composite solid electrolyte membrane. The technical solution adopted is summarized as follows: first, electrospinning and high-temperature heat treatment technology are used to prepare high-valent metal atoms rich in oxygen vacancies doped with rare earth metal oxides as inorganic fillers for composite solid electrolytes; then, the oxides are dispersed in a solvent with lithium salts and polymer matrices to obtain different electrospinning precursor solutions, and multilayer composite solid electrolyte nanofiber membranes are spun on a receiver in sequence. The multilayer composite solid electrolyte nanofiber membrane has good compatibility with lithium metal and can be used with high-voltage positive electrode materials, thereby improving the energy density of lithium batteries and broadening the electrochemical window. At the same time, the ultra-thin interface modification layer can effectively avoid problems such as increased volume, weight and total resistance of the battery.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides a method for preparing a multilayer composite solid electrolyte membrane, comprising the following steps:

[0007] (1) Preparation of inorganic fillers

[0008] A high-valent metal salt, a rare earth metal salt and a low decomposition temperature polymer are mixed and dissolved in a solvent A in a certain mass ratio to obtain a spinning precursor solution B, and then spun by electrostatic spinning to obtain a precursor fiber membrane layer; after calcination at 200-500° C., annealing is performed to obtain a high-valent metal atom-doped rare earth metal oxide inorganic filler.

[0009] Wherein, the high-valent metal salt is selected from any one of gadolinium nitrate, ytterbium nitrate, and yttrium acetate;

[0010] The rare earth metal salt is selected from one of lanthanum chloride and cerium nitrate hexahydrate;

[0011] The low decomposition temperature polymer is selected from one of polyvinyl pyrrolidone, polymethyl methacrylate and polystyrene;

[0012] The mass ratio of high-valent metal salt to rare earth metal salt is 1:1-20, the mass ratio of total metal salt mass to low decomposition temperature polymer is 1:1-4, and the concentration of low decomposition temperature polymer is 8wt-15wt%.

[0013] Solvent A is selected from one of dimethyl sulfoxide, N,N-dimethylacetamide and N,N-dimethylformamide;

[0014] The electrospinning conditions were as follows: voltage 12-20 kV, humidity 10-30%, and distance from spinning needle to receiver 8-24 cm;

[0015] During calcination, the precursor fiber membrane layer is placed in a tubular furnace, heated at a rate of 5° C. per minute in an air atmosphere, and annealed after constant temperature calcination at a temperature of 200 to 500° C. for 2 to 3 hours.

[0016] (2) Preparation of multilayer composite solid electrolyte fiber membrane

[0017] 2-1 Preparation of spinning precursor solution

[0018] The lithium salt and the inorganic filler prepared in step (1) are dissolved in an organic solvent C, and the fluorine-containing polymer is dissolved therein to obtain a spinning precursor solution D; the lithium salt and the inorganic filler prepared in step (1) are dissolved in an organic solvent E, and the polar polymer is dissolved therein to obtain a spinning precursor solution F.

[0019] The content of the fluorine-containing polymer in the spinning precursor solution D is 6wt-12wt%, the mass ratio of the lithium salt to the fluorine-containing polymer is 1:1-5, and the mass ratio of the inorganic filler to the lithium salt is 1:1-5;

[0020] In the spinning precursor solution F, the content of the polar polymer is 3wt-7wt%, the mass ratio of the lithium salt to the polar polymer is 1:1-5, and the mass ratio of the inorganic filler to the lithium salt is 1:1-5.

[0021] The lithium salt is selected from any one or more combinations of lithium trifluoromethanesulfonate, lithium nitrate, lithium hexafluorophosphate, and lithium borohydride;

[0022] The organic solvent C is selected from any one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone;

[0023] The fluorine-containing polymer is selected from any one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, and fluororubber;

[0024] The organic solvent E is selected from any one of acetonitrile, N,N-dimethylformamide and dimethyl sulfoxide;

[0025] The polar polymer is selected from one of polyethylene oxide, polyacrylonitrile and polyimide.

[0026] 2-2 Three-layer composite solid electrolyte fiber membrane spinning

[0027] Using spinning precursor solution D as raw material and peelable paper as receiver, an electrostatic spinning process is used to spin a fluorine-containing composite solid electrolyte interface modified fiber membrane layer (the membrane layer thickness is controlled at 5 microns to 20 microns); then, using the fluorine-containing composite solid electrolyte interface modified fiber membrane layer as a receiver, using spinning precursor solution F to cover it by electrostatic spinning, and obtaining a double-layer composite solid electrolyte fiber membrane layer with a "Janus" structure (thickness is 80 to 150 microns); finally, using the double-layer composite solid electrolyte fiber membrane layer as a receiver, using spinning precursor solution D to cover it by electrostatic spinning (thickness is also 5 microns to 20 microns), a three-layer "sandwich" structure composite solid electrolyte fiber membrane is obtained. After removing the peelable paper, the multi-layer composite solid electrolyte fiber membrane is obtained after vacuum drying at 60°C for 2 to 5 hours.

[0028] The electrospinning conditions are as follows: voltage 12-20 kV, humidity 10-30%, and distance from the spinning needle to the receiver 8-24 cm.

[0029] In the second aspect of the present invention, a multilayer composite solid electrolyte membrane is provided, which is prepared by the method described above. In the specific implementation method of the present invention, the composite solid electrolyte membranes with different numbers of layers constructed by different types of high-valent metal atoms doped with rare earth metal oxide inorganic fillers are tested for ion conductivity and specific capacity retention rate. The results show that the short rod-shaped one-dimensional nanofiber inorganic filler prepared by the method of the present invention can effectively accelerate the transmission rate of lithium ions. At the same time, the electrostatic spinning technology enhances the mechanical strength and chemical stability of the multilayer composite solid electrolyte membrane, has a higher specific capacity retention rate in the charge and discharge cycle, and greatly prolongs the cycle life of the lithium metal battery.

[0030] The third aspect of the present invention provides the use of a multilayer composite solid electrolyte membrane in the preparation of a solid-state lithium-ion battery.

[0031] In a fourth aspect, the present invention provides a solid-state lithium-ion battery, the electrolyte of which is the multilayer composite solid-state electrolyte membrane described above.

[0032] Beneficial technical effects of the present invention:

[0033] (1) The high-valent metal atom-doped rare earth metal oxide inorganic filler prepared by electrospinning and high-temperature heat treatment technology can reduce the crystallinity of the polymer and provide more transmission channels for lithium ions. On the other hand, its abundant oxygen vacancies interact with lithium salts through Lewis acid-base interactions, promoting the dissociation of lithium salts to increase the number of free Li ions and significantly improve ionic conductivity. At the same time, the one-dimensional short rod-shaped nanofibers can form a Li ion transmission percolation network, providing a high-speed channel for Li ion transmission.

[0034] (2) In the multi-layer structure composite solid polymer electrolyte prepared by the present invention, the electrochemical performance of the fluorine-containing composite electrolyte interface modification layer is stable. It can contact with the positive electrode to form the positive electrode electrolyte interface CEI, effectively enhancing the antioxidant capacity of the composite solid electrolyte, widening the electrochemical window, and perfectly matching with the high-voltage positive electrode materials on the market, significantly improving the energy density of the solid-state battery and meeting the actual application needs; it can also contact with the negative electrode to form the negative electrode electrolyte interface SEI. The excellent mechanical strength of the fluorine-containing polymer can effectively inhibit the lithium dendrites from piercing the electrolyte and causing battery short circuit and other safety problems, while reducing the concentration difference polarization and reaction by-products in the battery system, preventing the uneven deposition of metallic lithium, thereby ensuring the cycle stability of the solid-state battery.

[0035] (3) The electrospinning strategy proposed in the present invention for preparing multilayer composite solid electrolytes can not only construct a three-dimensional skeleton structure with precisely controlled porosity, form a continuous ion transmission channel, and improve the ion conductivity of the electrolyte, but also easily regulate the thickness of the multilayer composite nanofiber membrane electrolyte, so that it has excellent interfacial compatibility, reduces interfacial resistance, and enhances interfacial stability. It greatly simplifies the preparation process and improves production efficiency, providing more effective solutions and innovative technologies for the rational design and preparation of multilayer composite solid electrolytes that are simultaneously stable and compatible with high-voltage positive electrodes and lithium metal negative electrodes.

[0036] The projects on which this invention is based are as follows: Project type: Shanghai Science and Technology Commission, Basic Research Special Zone Plan; Project number: 22T01400100-18; Project name: Design, preparation and application of key materials for solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a flowchart of the preparation method of the multilayer composite solid electrolyte in the present invention;

[0038] Figure 2 This is a field emission scanning electron microscope photo of the inorganic filler doped with rare earth metal oxides with high-valent metal atoms constructed in Example 1;

[0039] Figure 3 The ionic conductivity of the multilayer composite solid electrolyte constructed in Example 1 at different temperatures;

[0040] Figure 4 The capacity and coulombic efficiency of the multilayer composite solid electrolyte lithium metal battery constructed in Example 1 during the charge and discharge cycle. DETAILED DESCRIPTION

[0041] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0042] Figure 1 The preparation process of the multilayer composite solid electrolyte membrane of the present invention is shown, which mainly includes two processes: (1) synthesizing high-valent metal atoms rich in oxygen vacancies and doped with rare earth metal oxide inorganic fillers; (2) preparing a "sandwich" multilayer structure formed by a fluorine-containing polymer interface modified composite solid electrolyte, a polar polymer composite solid electrolyte, and a fluorine-containing polymer interface modified composite solid electrolyte.

[0043] The present invention explores the construction of inorganic fillers of different raw material types and the multi-layer composite solid electrolyte membrane constructed therefrom, for details, see the following Examples 1 to 6.

[0044] Example 1

[0045] The specific steps of the preparation method of the multilayer composite solid electrolyte of this embodiment are as follows:

[0046] (1) Electrospinning and high-temperature heat treatment techniques are used to prepare rare earth metal oxides doped with high-valent metal atoms rich in oxygen vacancies as inorganic fillers for composite solid electrolytes

[0047] a. Dissolve ytterbium nitrate, cerium nitrate hexahydrate and polyvinyl pyrrolidone in N,N-dimethylformamide in a certain mass ratio to obtain a spinning precursor solution B. The mass ratio of ytterbium nitrate to cerium nitrate hexahydrate is controlled to be 1:4, the mass ratio of the total mass of ytterbium nitrate and cerium nitrate hexahydrate to polyvinyl pyrrolidone is 1:1.25, and the content of polyvinyl pyrrolidone is 12wt%;

[0048] b. Use spinning precursor solution B, aluminum foil as receiver, and spin through an electrospinning machine to obtain a precursor fiber membrane layer, and the membrane layer thickness is controlled at 200 microns. The electrospinning conditions are as follows: voltage is 18kV, humidity is 10%, and the distance from the spinning needle to the receiver is 20cm;

[0049] c. The precursor fiber membrane layer is placed in a tubular furnace, heated to 250°C at a rate of 5°C per minute in an air atmosphere, and then calcined at a constant temperature for 2 hours. Then, the temperature is increased to 400°C at a rate of 5°C per minute and calcined at a constant temperature for 3 hours to obtain ytterbium-doped cerium oxide inorganic filler.

[0050] Characterization was performed by field emission scanning electron microscopy, such as Figure 2 As shown, it can be seen that the inorganic filler is a short rod-shaped one-dimensional hollow nanotube. This hollow structure has a large specific surface area, and its surface is rich in oxygen vacancies and positively charged active sites. It promotes the dissociation of lithium salts through Lewis acid-base action, thereby generating more lithium ions. At the same time, the one-dimensional nanotube can form a lithium ion transport percolation network, providing a high-speed channel for the transport of lithium ions, and significantly improving the conductivity of the composite electrolyte.

[0051] (2) Electrospinning to produce a multi-layer composite solid electrolyte nanofiber membrane

[0052] a. dissolving lithium trifluoromethanesulfonate and ytterbium-doped cerium oxide inorganic filler into N, N-dimethylformamide, and then dissolving fluororubber into the above solution to obtain a spinning precursor solution D, wherein the fluororubber content is controlled to be 8wt%, the mass ratio of lithium trifluoromethanesulfonate to fluororubber is 1:2, and the mass ratio of ytterbium-doped cerium oxide inorganic filler to lithium trifluoromethanesulfonate is 1:2;

[0053] b. dissolving lithium trifluoromethanesulfonate and ytterbium-doped cerium oxide inorganic filler into acetonitrile, and then dissolving polyethylene oxide into the above solution to obtain a spinning precursor solution F, wherein the polyethylene oxide content is controlled to be 5wt%, the mass ratio of lithium trifluoromethanesulfonate to polyethylene oxide is 1:2, and the mass ratio of ytterbium-doped cerium oxide to lithium trifluoromethanesulfonate is 1:2;

[0054] c. Using spinning precursor solution D, oil film paper as a receiver, spinning through an electrospinning machine to obtain a fluororubber composite solid electrolyte interface modified fiber membrane layer, the thickness of which is controlled at 10 microns; then, using the fluororubber composite solid electrolyte interface modified fiber membrane layer as a receiver, using spinning precursor solution F through electrospinning to cover the interface modified precursor fiber membrane layer, and finally, on the surface of the solid electrolyte precursor fiber membrane layer, using spinning precursor solution D through electrospinning to cover the solid electrolyte precursor fiber membrane layer, to obtain a "sandwich" structure composite solid electrolyte fiber membrane, the thickness of which is controlled at 110 microns. After removing the oil film paper, put it in a vacuum drying oven at 60°C and dry it for 4 hours to remove the residual solvent, and obtain a three-layer composite solid electrolyte. The above electrospinning conditions are: voltage of 17kV, humidity of 10%, and the distance from the spinning needle to the receiver is 18cm.

[0055] The composite solid electrolyte nanofiber membrane constructed in this example was used to construct a lithium metal battery, and the battery was tested for conductivity and charge-discharge cycle at different temperatures. The results are as follows: Figure 3 As shown in Figure 2, at 30°C, the conductivity of the multilayer composite solid electrolyte can reach 1.12×10 -4 S / cm. In addition, according to Figure 4 It is shown that the charge-discharge specific capacity of the multilayer composite solid-state lithium metal battery can reach 135mAh / g at a high current density of 2C, and the capacity retention rate is about 99.6% after 50 cycles. This shows that the construction scheme of this embodiment effectively enhances the interface stability and cycle stability between the electrode and the electrolyte, so that the device can still operate efficiently and stably at a high current density, showing excellent electrochemical performance.

[0056] Example 2

[0057] The preparation method of the multilayer composite solid electrolyte of this embodiment comprises the following steps:

[0058] (1) Electrospinning and high-temperature heat treatment techniques are used to prepare rare earth metal oxides doped with high-valent metal atoms rich in oxygen vacancies as inorganic fillers for composite solid electrolytes

[0059] a. dissolving and mixing gadolinium nitrate, cerium nitrate hexahydrate and polymethyl methacrylate in N,N-dimethylacetamide in a certain mass ratio to obtain a spinning precursor solution B, wherein the mass ratio of gadolinium nitrate to cerium nitrate hexahydrate is controlled to be 1:10, the mass ratio of the total mass of gadolinium nitrate and cerium nitrate hexahydrate to polymethyl methacrylate is 1:2, and the content of polymethyl methacrylate is 10wt%;

[0060] b. Using spinning precursor solution B, aluminum foil as a receiver, and spinning through an electrospinning machine to obtain a precursor fiber film layer, the thickness of which is controlled at 200 microns. The electrospinning conditions are as follows: voltage of 16 kV, humidity of 10%, and the distance from the spinning needle to the receiver of 18 cm;

[0061] c. The precursor fiber membrane layer is placed in a tubular furnace, heated to 300°C at a rate of 5°C per minute in an air atmosphere and calcined at a constant temperature for 2 hours, and then heated to 400°C at a rate of 5°C per minute and calcined at a constant temperature for 3 hours to obtain a gadolinium-doped cerium oxide inorganic filler.

[0062] (2) Electrospinning to produce a multi-layer composite solid electrolyte nanofiber membrane

[0063] a. dissolving lithium trifluoromethane sulfonate and gadolinium-doped cerium oxide inorganic filler into N, N-dimethylformamide, and then dissolving polyvinylidene fluoride into the above solution to obtain a spinning precursor solution D, wherein the polyvinylidene fluoride content is controlled to be 10wt%, the mass ratio of lithium trifluoromethane sulfonate to polyvinylidene fluoride is 1:3, and the mass ratio of gadolinium-doped cerium oxide inorganic filler to lithium trifluoromethane sulfonate is 1:3;

[0064] b. dissolving lithium trifluoromethane sulfonate and gadolinium-doped cerium oxide inorganic filler into acetonitrile, and then dissolving polyethylene oxide into the above solution to obtain a spinning precursor solution F, wherein the polyethylene oxide content is controlled to be 5wt%, the mass ratio of lithium trifluoromethane sulfonate to polyethylene oxide is 1:3, and the mass ratio of gadolinium-doped cerium oxide to lithium trifluoromethane sulfonate is 1:3;

[0065] c. Using spinning precursor solution D, oil film paper as a receiver, spinning through an electrospinning machine to obtain a polyvinylidene fluoride composite solid electrolyte interface modified fiber membrane layer, the thickness of which is controlled at 15 microns; then, using the polyvinylidene fluoride composite solid electrolyte interface modified fiber membrane layer as a receiver, using spinning precursor solution F through electrospinning, covering the interface modified precursor fiber membrane layer, to obtain an asymmetric "Janus" structure composite solid electrolyte fiber membrane layer, the thickness of which is controlled at 100 microns. After removing the oil film paper, put it in a vacuum drying oven at 60°C and dry it for 3 hours to remove the residual solvent, and obtain a double-layer composite solid electrolyte. The above electrospinning conditions are: voltage of 18kV, humidity of 10%, and the distance from the spinning needle to the receiver is 20cm.

[0066] Example 3

[0067] The method for preparing the multilayer composite solid electrolyte provided in this embodiment comprises the following steps:

[0068] (1) Electrospinning and high-temperature heat treatment techniques are used to prepare rare earth metal oxides doped with high-valent metal atoms rich in oxygen vacancies as inorganic fillers for composite solid electrolytes

[0069] a. Dissolve yttrium acetate, lanthanum chloride and polyvinyl pyrrolidone in N, N-dimethylformamide in a certain mass ratio to obtain a spinning precursor solution B, wherein the mass ratio of yttrium acetate to lanthanum chloride is controlled to be 1:6, the mass ratio of the total mass of yttrium acetate and lanthanum chloride to polyvinyl pyrrolidone is 1:2.5, and the content of polyvinyl pyrrolidone is 8wt%;

[0070] b. Using spinning precursor solution B, aluminum foil as a receiver, and spinning through an electrospinning machine to obtain a precursor fiber film layer; the film thickness is controlled at 250 microns, and the above electrospinning conditions are: voltage of 18kV, humidity of 10%, and the distance from the spinning needle to the receiver is 23cm;

[0071] c. The precursor fiber membrane layer is placed in a tubular furnace, heated to 250°C at a rate of 5°C per minute in an air atmosphere, and then calcined at a constant temperature for 2 hours. Then, the temperature is increased to 400°C at a rate of 5°C per minute and calcined at a constant temperature for 3 hours to obtain yttrium-doped lanthanum oxide inorganic filler.

[0072] (2) Electrospinning to produce a multi-layer composite solid electrolyte nanofiber membrane

[0073] a. dissolving lithium nitrate and yttrium-doped lanthanum oxide inorganic filler into N-methylpyrrolidone, and then dissolving polyvinylidene fluoride into the above solution to obtain a spinning precursor solution D, wherein the polyvinylidene fluoride content is controlled to be 12wt%, the mass ratio of lithium nitrate to polyvinylidene fluoride is 1:2.5, and the mass ratio of yttrium-doped lanthanum oxide inorganic filler to lithium trinitrate is 1:2.5;

[0074] b. dissolving lithium nitrate and yttrium-doped lanthanum oxide inorganic filler into N, N-dimethylformamide, and then dissolving polyacrylonitrile into the above solution to obtain a spinning precursor solution F, wherein the polyacrylonitrile content is controlled to be 6wt%, the mass ratio of lithium nitrate to polyacrylonitrile is 1:2.5, and the mass ratio of yttrium-doped lanthanum oxide to lithium nitrate is 1:2.5;

[0075] c. Using spinning precursor solution D, oil film paper as a receiver, spinning through an electrospinning machine to obtain a polyvinylidene fluoride composite solid electrolyte interface modified fiber membrane layer, the thickness of which is controlled at 8 microns; then, using the polyvinylidene fluoride composite solid electrolyte interface modified fiber membrane layer as a receiver, using spinning precursor solution F through electrospinning to cover the interface modified precursor fiber membrane layer, and finally, on the surface of the solid electrolyte precursor fiber membrane layer, using spinning precursor solution D through electrospinning to cover the solid electrolyte precursor fiber membrane layer, to obtain a "sandwich" structure composite solid electrolyte fiber membrane, the thickness of which is controlled at 100 microns. After removing the oil film paper, put it in a vacuum drying oven at 60°C and dry it for 4 hours to remove the residual solvent, and obtain a three-layer composite solid electrolyte. The above electrospinning conditions are: voltage of 16kV, humidity of 20%, and the distance from the spinning needle to the receiver is 19cm.

[0076] Example 4

[0077] The method for preparing the multilayer composite solid electrolyte provided in this embodiment comprises the following steps:

[0078] (1) Electrospinning and high-temperature heat treatment techniques are used to prepare rare earth metal oxides doped with high-valent metal atoms rich in oxygen vacancies as inorganic fillers for composite solid electrolytes

[0079] a. Dissolve ytterbium nitrate, lanthanum chloride and polystyrene in dimethyl sulfoxide in a certain mass ratio to obtain a spinning precursor solution B, wherein the mass ratio of ytterbium nitrate to lanthanum chloride is controlled to be 1:15, the mass ratio of the total mass of ytterbium nitrate and lanthanum chloride to polystyrene is 1:4, and the polystyrene content is 8wt%;

[0080] b. Using spinning precursor solution B, aluminum foil as a receiver, and spinning through an electrospinning machine to obtain a precursor fiber film layer; the film thickness is controlled at 300 microns, and the above electrospinning conditions are: voltage of 16kV, humidity of 10%, and the distance from the spinning needle to the receiver is 22cm;

[0081] c. The precursor fiber membrane layer is placed in a tubular furnace, heated to 300°C at a rate of 5°C per minute in an air atmosphere, and then calcined at a constant temperature for 3 hours, followed by annealing to obtain an ytterbium-doped lanthanum oxide inorganic filler.

[0082] (2) Electrospinning to produce a multi-layer composite solid electrolyte nanofiber membrane

[0083] a. dissolving lithium hexafluorophosphate and ytterbium-doped lanthanum oxide inorganic filler into N, N-dimethylacetamide, and then dissolving fluororubber into the above solution to obtain a spinning precursor solution D, wherein the fluororubber content is controlled to be 11wt%, the mass ratio of lithium hexafluorophosphate to fluororubber is 1:1.5, and the mass ratio of ytterbium-doped lanthanum oxide inorganic filler to lithium hexafluorophosphate is 1:1.5;

[0084] b. dissolving lithium hexafluorophosphate and ytterbium-doped lanthanum oxide inorganic filler into dimethyl sulfoxide, and then dissolving polyacrylonitrile into the above solution to obtain a spinning precursor solution F, wherein the polyacrylonitrile content is controlled to be 6wt%, the mass ratio of lithium hexafluorophosphate to polyacrylonitrile is 1:1.5, and the mass ratio of ytterbium-doped lanthanum oxide to lithium hexafluorophosphate is 1:1.5;

[0085] c. Using spinning precursor solution D, oil film paper as a receiver, spinning through an electrospinning machine to obtain a fluororubber composite solid electrolyte interface modified fiber membrane layer, the thickness of which is controlled at 5 microns; then, using the fluororubber composite solid electrolyte interface modified fiber membrane layer as a receiver, using spinning precursor solution F through electrospinning, covering the interface modified precursor fiber membrane layer, to obtain an asymmetric "Janus" structure composite solid electrolyte fiber membrane layer, the thickness of which is controlled at 80 microns. After removing the oil film paper, put it in a vacuum drying oven at 60°C and dry it for 2h to remove the residual solvent to obtain a double-layer composite solid electrolyte. The above electrospinning conditions are: voltage of 19kV, humidity of 10%, and the distance from the spinning needle to the receiver is 18cm.

[0086] Example 5

[0087] The method for preparing the multilayer composite solid electrolyte provided in this embodiment comprises the following steps:

[0088] (1) Electrospinning and high-temperature heat treatment techniques are used to prepare rare earth metal oxides doped with high-valent metal atoms rich in oxygen vacancies as inorganic fillers for composite solid electrolytes

[0089] a. Dissolve yttrium acetate, cerium nitrate hexahydrate and polystyrene in N, N-dimethylacetamide in a certain mass ratio to obtain a spinning precursor solution B, wherein the mass ratio of yttrium acetate to cerium nitrate hexahydrate is controlled to be 1:8, the mass ratio of the total mass of yttrium acetate and cerium nitrate hexahydrate to polystyrene is 1:3, and the polystyrene content is 14wt%;

[0090] b. Use spinning precursor solution B, aluminum foil as receiver, and spin through an electrospinning machine to obtain a precursor fiber membrane layer, and the membrane layer thickness is controlled at 300 microns. The electrospinning conditions are as follows: voltage is 17kV, humidity is 20%, and the distance from the spinning needle to the receiver is 20cm;

[0091] c. The precursor fiber membrane layer is placed in a tubular furnace, heated to 300°C at a rate of 5°C per minute in an air atmosphere, and then calcined at a constant temperature for 2 hours and annealed to obtain a yttrium-doped cerium oxide inorganic filler.

[0092] (2) Electrospinning to produce a multi-layer composite solid electrolyte nanofiber membrane

[0093] a. dissolving lithium borohydride and yttrium-doped cerium oxide inorganic filler into N-methylpyrrolidone, and then dissolving polyvinylidene fluoride-hexafluoropropylene into the above solution to obtain a spinning precursor solution D, wherein the polyvinylidene fluoride-hexafluoropropylene content is controlled to be 10wt%, the mass ratio of lithium borohydride to polyvinylidene fluoride-hexafluoropropylene is 1:3, and the mass ratio of yttrium-doped cerium oxide inorganic filler to lithium borohydride is 1:3;

[0094] b. dissolving lithium borohydride and yttrium-doped cerium oxide inorganic filler into dimethyl sulfoxide, and then dissolving polyimide into the above solution to obtain a spinning precursor solution F, wherein the polyimide content is controlled to be 4wt%, the mass ratio of lithium borohydride to polyimide is 1:3, and the mass ratio of yttrium-doped cerium oxide to lithium borohydride is 1:3;

[0095] c. Using spinning precursor solution D, oil film paper as a receiver, through electrospinning machine spinning, obtain polyvinylidene fluoride-hexafluoropropylene composite solid electrolyte interface modified fiber membrane layer, the membrane thickness is controlled at 20 microns; then, using polyvinylidene fluoride-hexafluoropropylene composite solid electrolyte interface modified fiber membrane layer as a receiver, using spinning precursor solution F through electrospinning, covering the interface modified precursor fiber membrane layer, to obtain a double-layer asymmetric structure of "Janus" composite solid electrolyte fiber membrane layer, the thickness of which is controlled at 130 microns. After removing the oil film paper, put it in a vacuum drying oven at 60°C and dry it for 4 hours to remove the residual solvent, and obtain a double-layer composite solid electrolyte. The above electrospinning conditions are: voltage of 17.5kV, humidity of 10%, and the distance from the spinning needle to the receiver is 21cm.

[0096] Example 6

[0097] The preparation method of the multilayer composite solid electrolyte in this embodiment comprises the following steps:

[0098] (1) Electrospinning and high-temperature heat treatment techniques are used to prepare rare earth metal oxides doped with high-valent metal atoms rich in oxygen vacancies as inorganic fillers for composite solid electrolytes

[0099] a. dissolving and mixing gadolinium nitrate, lanthanum chloride and polyvinyl pyrrolidone in N,N-dimethylformamide in a certain mass ratio to obtain a spinning precursor solution B, wherein the mass ratio of gadolinium nitrate to lanthanum chloride is controlled to be 1:15, the mass ratio of the total mass of yttrium acetate and lanthanum chloride to polyvinyl pyrrolidone is 1:3, and the content of polyvinyl pyrrolidone is 12wt%;

[0100] b. Using spinning precursor solution B, aluminum foil as a receiver, and spinning through an electrospinning machine to obtain a precursor fiber film layer; the film thickness is controlled at 300 microns, and the above electrospinning conditions are: voltage of 17kV, humidity of 10%, and the distance from the spinning needle to the receiver is 22cm;

[0101] c. The precursor fiber membrane layer is placed in a tubular furnace, heated to 250°C at a rate of 5°C per minute in an air atmosphere, and then calcined at a constant temperature for 2 hours. Then, the temperature is increased to 400°C at a rate of 5°C per minute and calcined at a constant temperature for 3 hours to obtain a gadolinium-doped lanthanum oxide inorganic filler.

[0102] (2) Electrospinning to produce a multi-layer composite solid electrolyte nanofiber membrane

[0103] a. dissolving lithium nitrate and gadolinium-doped lanthanum oxide inorganic filler into N-methylpyrrolidone, and then dissolving polyvinylidene fluoride-hexafluoropropylene into the above solution to obtain a spinning precursor solution D, wherein the content of polyvinylidene fluoride-hexafluoropropylene is controlled to be 9wt%, the mass ratio of lithium nitrate to polyvinylidene fluoride-hexafluoropropylene is 1:2, and the mass ratio of gadolinium-doped lanthanum oxide inorganic filler to lithium nitrate is 1:1.5;

[0104] b. dissolving lithium nitrate and gadolinium-doped lanthanum oxide inorganic filler into acetonitrile, and then dissolving polyethylene oxide into the above solution to obtain a spinning precursor solution F, wherein the polyethylene oxide content is controlled to be 5wt%, the mass ratio of lithium nitrate to polyethylene oxide is 1:2, and the mass ratio of yttrium-doped lanthanum oxide to lithium nitrate is 1:1.5;

[0105] c. Using spinning precursor solution D, oil film paper as a receiver, spinning through an electrospinning machine to obtain a polyvinylidene fluoride-hexafluoropropylene composite solid electrolyte interface modified fiber membrane layer, the thickness of which is controlled at 10 microns; then, using the polyvinylidene fluoride-hexafluoropropylene composite solid electrolyte interface modified fiber membrane layer as a receiver, using spinning precursor solution F through electrospinning to cover the interface modified precursor fiber membrane layer, and finally, on the surface of the solid electrolyte precursor fiber membrane layer, using spinning precursor solution D through electrospinning to cover the solid electrolyte precursor fiber membrane layer, to obtain a "sandwich" structure composite solid electrolyte fiber membrane, the thickness of which is controlled at 120 microns. After removing the oil film paper, put it in a vacuum drying oven at 60°C and dry it for 4 hours to remove the residual solvent, and obtain a three-layer composite solid electrolyte. The above electrospinning conditions are: voltage of 18.5kV, humidity of 20%, and the distance from the spinning needle to the receiver is 18cm.

[0106] Comparative Example 1

[0107] Using the raw materials of Example 1, a single-layer composite solid electrolyte was prepared by tape casting, comprising the following steps:

[0108] (1) Using glass sheet casting method and high temperature heat treatment technology to prepare high-valent metal atoms rich in oxygen vacancies doped rare earth metal oxides as inorganic fillers for composite solid electrolytes

[0109] a. The same as in Example 1, to obtain a casting solution B;

[0110] b. Cast the casting liquid B evenly on a flat glass plate to form a film, and vacuum dry it for 24 hours. After the solvent is completely evaporated, a precursor film layer is obtained with a thickness controlled to be 200 microns.

[0111] c. As in Example 1, an inorganic filler was obtained;

[0112] (2) Preparation of composite solid electrolyte by glass plate casting method

[0113] a. dissolving lithium trifluoromethanesulfonate and the inorganic filler obtained in (1) into acetonitrile, and then dissolving polyethylene oxide into the above solution to obtain a casting solution F, wherein the polyethylene oxide content is controlled to be 5wt%, the mass ratio of lithium trifluoromethanesulfonate to polyethylene oxide is 1:2, and the mass ratio of the inorganic filler to lithium trifluoromethanesulfonate is 1:2;

[0114] b. The casting solution F was uniformly cast on a flat glass plate to form a film, and then vacuum dried at 60°C for 12 hours. After the solvent was completely evaporated, a composite solid electrolyte membrane layer was obtained with a thickness controlled to be 100 microns.

[0115] In addition, the electrochemical performance of the composite solid-state lithium metal batteries constructed in Examples 1 to 6 and Comparative Example 1 was tested under dynamic and static conditions. The specific test results are shown in Table 1:

[0116] Table 1 Test results of the integrated composite solid-state lithium metal batteries constructed in Examples 1 to 6 and Comparative Example 1

[0117]

[0118] Comparing the data shown in Table 1, the fiber membrane spun by the ytterbium-doped cerium oxide inorganic filler and the fluororubber interface modification layer system exhibits higher ionic conductivity and cycle stability. Compared with Comparative Example 1, the short rod-shaped one-dimensional nanofiber inorganic filler spun by electrospinning can effectively accelerate the transmission rate of lithium ions. At the same time, the electrospinning technology enhances the mechanical strength and chemical stability of the multilayer composite solid electrolyte membrane, and has a higher specific capacity retention rate in the charge and discharge cycle, greatly extending the cycle life of the lithium metal battery.

[0119] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.

Claims

1. A method for preparing a multilayer composite solid electrolyte membrane, characterized in that: The steps include: (1) Preparation of inorganic fillers A high-valent metal salt, a rare earth metal salt and a low decomposition temperature polymer are mixed and dissolved in a solvent A according to a certain mass ratio to obtain a spinning precursor solution B, and the solution is spun by electrostatic spinning to obtain a precursor fiber membrane layer; After calcination at 200-500°C and annealing, a high-valent metal atom-doped rare earth metal oxide inorganic filler is obtained; (2) Preparation of multilayer composite solid electrolyte fiber membrane Dissolving the lithium salt and the inorganic filler prepared in step (1) into an organic solvent C, and then dissolving the fluorine-containing polymer therein to obtain a spinning precursor solution D; Dissolving the lithium salt and the inorganic filler prepared in step (1) into an organic solvent E, and then dissolving the polar polymer therein to obtain a spinning precursor solution F; Using spinning precursor solution D as raw material, an electrospinning process is adopted to obtain a fluorine-containing composite solid electrolyte interface modified fiber membrane layer; Then, the fluorine-containing composite solid electrolyte interface modified fiber membrane layer is used as a receiver, and a spinning precursor solution F is used to cover it by electrospinning to obtain a double-layer composite solid electrolyte fiber membrane layer; finally, the double-layer composite solid electrolyte fiber membrane layer is used as a receiver, and a spinning precursor solution D is used to cover it by electrospinning to obtain a three-layer composite solid electrolyte fiber membrane, and the multi-layer composite solid electrolyte fiber membrane is obtained after vacuum drying at 60°C.

2. The method for preparing a multilayer composite solid electrolyte membrane according to claim 1, characterized in that: in, In step (1), the high-valent metal salt is selected from any one of gadolinium nitrate, ytterbium nitrate, and yttrium acetate; The rare earth metal salt is selected from one of lanthanum chloride and cerium nitrate hexahydrate; The low decomposition temperature polymer is selected from one of polyvinyl pyrrolidone, polymethyl methacrylate and polystyrene; The mass ratio of the high-valent metal salt to the rare earth metal salt is 1:1-20, the mass ratio of the total mass of the metal salt to the low decomposition temperature polymer is 1:1-4, and the concentration of the low decomposition temperature polymer is 8wt%-15wt%.

3. The method for preparing a multilayer composite solid electrolyte membrane according to claim 1, characterized in that: in, In step (1), solvent A is selected from one of dimethyl sulfoxide, N,N-dimethylacetamide and N,N-dimethylformamide; The electrospinning conditions were as follows: voltage 12-20 kV, humidity 10-30%, and distance from spinning needle to receiver 8-24 cm; During calcination, the precursor fiber membrane layer is placed in a tubular furnace, heated at a rate of 5° C. per minute in an air atmosphere, and annealed after constant temperature calcination at a temperature of 200 to 500° C. for 2 to 3 hours.

4. The method for preparing a multilayer composite solid electrolyte membrane according to claim 1, characterized in that: in, In step (2), the content of the fluorine-containing polymer in the spinning precursor solution D is 6 wt % to 12 wt %, the mass ratio of the lithium salt to the fluorine-containing polymer is 1:1 to 5, and the mass ratio of the inorganic filler to the lithium salt is 1:1 to 5; In the spinning precursor solution F, the content of the polar polymer is 3wt-7wt%, the mass ratio of the lithium salt to the polar polymer is 1:1-5, and the mass ratio of the inorganic filler to the lithium salt is 1:1-5. The lithium salt is selected from any one or more combinations of lithium trifluoromethanesulfonate, lithium nitrate, lithium hexafluorophosphate, and lithium borohydride; The organic solvent C is selected from any one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone; The fluorine-containing polymer is selected from any one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, and fluororubber; The organic solvent E is selected from any one of acetonitrile, N,N-dimethylformamide, and dimethyl sulfoxide; The polar polymer is selected from one of polyethylene oxide, polyacrylonitrile and polyimide.

5. The method for preparing a multilayer composite solid electrolyte membrane according to claim 1, characterized in that: in, In step (2), the electrospinning conditions are: voltage 12-20 kV, humidity 10-30%, and the distance from the spinning needle to the receiver 8-24 cm; When preparing the fluorine-containing composite solid electrolyte interface modified fiber membrane layer, the peelable paper is used as the receiver, and the thickness of the membrane layer is controlled to be 5 microns to 20 microns; the thickness of the double-layer composite solid electrolyte fiber membrane layer is 80 to 150 microns; the thickness of the third layer of fluorine-containing composite solid electrolyte interface modified fiber membrane layer is also 5 microns to 20 microns; The three-layer composite solid electrolyte fiber membrane is vacuum dried at 60° C. for 2 to 5 hours to obtain the multi-layer composite solid electrolyte fiber membrane.

6. A multilayer composite solid electrolyte membrane, characterized in that: The method is prepared by any one of claims 1 to 5.

7. Use of the multilayer composite solid electrolyte membrane according to claim 6 in the preparation of solid-state lithium-ion batteries.

8. A solid-state lithium-ion battery, characterized in that: The electrolyte is the multilayer composite solid electrolyte membrane as claimed in claim 6.

Citation Information

Patent Citations

  • Preparation method of core-shell structure electrospinning nanofiber-ceramic nanowire-based all-solid-state composite electrolyte

    CN113745643A

  • Solid oxide battery composite nanofiber and preparation method thereof

    CN113957566A

  • Preparation method and application of double-layer composite solid electrolyte

    CN117423893A

  • Method for manufacturing metal oxide fiber

    JP2014080700A

  • Polymer electrolyte having multilayer structure,method for preparing the same and lithium secondarybattery employing the same

    KR1020010066272A

Cited By

  • Separator for lithium manganese primary battery, preparation method therefor, lithium manganese primary battery and electrical apparatus

    WO2026214784A1