Recycling method of lithium ion battery
By charging lithium-ion batteries to 60% state of charge, disassembling and burning electrode sheets, and converting lithium ions to carbonate, the method enhances lithium recovery and purity while being environmentally friendly.
Patent Information
- Application Number
- CN202411291263.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-03
AI Technical Summary
Existing lithium-ion battery recycling methods fail to effectively separate and recover lithium and other elements due to the mixing of positive and negative electrodes, leading to poor recovery rates and impurities, especially with copper elements, and involve complex processes that are not environmentally friendly.
A method involving charging lithium-ion batteries to at least 60% state of charge, disassembling to separate negative and positive electrode sheets, burning these components to produce an aqueous lithium ion solution, and using carbon dioxide to convert lithium ions into lithium carbonate, while avoiding the use of acids or alkalis.
Improves lithium recovery rates and purity of recovered salts, simplifies the process, and reduces environmental impact by minimizing the use of harmful chemicals.
Smart Images

Figure CN119069859A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a lithium ion battery recycling method, belonging to the technical field of lithium ion battery recycling. Background Art
[0002] Chinese patent document CN107196007B provides a method for recycling and reusing lithium batteries, which mechanically crushes lithium batteries, washes with organic solvents, separates them by air flow grinding, soaks them in sulfuric acid and hydrogen peroxide solutions, and then uses alkaline solution precipitation to recover different ions in batches, first recovers non-necessary positive electrode materials such as iron, copper, and aluminum in batches, then recovers cobalt, nickel, and manganese in ternary positive electrode materials in batches, and finally recovers lithium ions. It can better separate various elements, facilitate the re-proportioning and adjustment of the ratio of nickel, cobalt, manganese, and lithium for the processing of ternary materials, increase the yield of each element, and also improve the purity of recovered Co.
[0003] However, the above-mentioned lithium battery recycling and reuse method still has some defects. For example, in the process of battery recycling, the positive and negative electrodes are not considered to be classified before the corresponding recycling, which leads to poor actual recycling effect. The purity of the samples actually recovered (such as lithium salts) does not meet the use requirements. In addition, since the material of the negative electrode matrix is generally copper, the separated samples are easily mixed with copper elements. In the process of battery recycling, the battery needs to undergo a corresponding discharge process, as well as a corresponding water immersion and crushing process. There is a large amount of unnecessary mixing, which increases the difficulty of recycling. Summary of the invention
[0004] The present invention provides a lithium ion battery recovery method, which effectively improves the recovery rate of lithium and the purity of recovered lithium salts, and has a simple process flow, convenient operation and environmental friendliness.
[0005] The present invention provides a lithium ion battery recycling method, comprising: charging the lithium ion battery to make the state of charge of the lithium ion battery reach at least 60%; disassembling the charged lithium ion battery to separate the negative electrode sheet, the diaphragm and the positive electrode sheet; burning the negative electrode sheet and the diaphragm, dissolving the combustion product in water, filtering to obtain an aqueous solution containing lithium ions and a filter residue; and separating lithium salts from the aqueous solution containing lithium ions.
[0006] Optionally, the lithium-ion battery is charged so that the state of charge of the lithium-ion battery reaches at least 75%.
[0007] Optionally, the lithium-ion battery is charged so that the state of charge of the lithium-ion battery reaches at least 105%.
[0008] Optionally, during the combustion process, an alkaline solution is used to absorb the exhaust gas generated during the combustion process.
[0009] Optionally, the process of burning the negative electrode plate and the separator includes: contacting the mixture of the negative electrode plate and the separator with water for burning.
[0010] Optionally, the lithium salt comprises lithium carbonate.
[0011] Optionally, the process of separating lithium salt from the aqueous solution containing lithium ions includes: introducing carbon dioxide into the aqueous solution containing lithium ions to convert lithium ions in the aqueous solution containing lithium ions into lithium carbonate, and then performing dehydration treatment to obtain the lithium salt.
[0012] Optionally, the process of separating lithium salt from the aqueous solution containing lithium ions includes: introducing carbon dioxide into the aqueous solution containing lithium ions until the pH of the solution is stable, stopping the introduction of carbon dioxide, and then performing the dehydration treatment to obtain the lithium salt.
[0013] Optionally, the process of introducing carbon dioxide into the aqueous solution containing lithium ions comprises: concentrating the aqueous solution containing lithium ions into a concentrated solution having a lithium hydroxide concentration of 15% to 22%, and then introducing carbon dioxide into the concentrated solution.
[0014] Optionally, the method further comprises: kneading and sieving the positive electrode sheet in sequence to obtain a positive electrode current collector material and a lithium-deficient positive electrode material; and mixing the lithium-deficient positive electrode material and lithium hydroxide and sintering the mixture to obtain a positive electrode material.
[0015] The present invention provides a lithium ion battery recycling method. The recycling method charges the lithium ion battery until its state of charge reaches at least 60%, then disassembles it to separate the negative electrode sheet, the diaphragm and the positive electrode sheet, burns the negative electrode sheet and the diaphragm together, dissolves the combustion product in water, filters it, and obtains an aqueous solution containing lithium ions. Lithium salts with high purity are separated from the aqueous solution containing lithium ions, which is beneficial to improving the recovery rate of lithium elements in lithium ion batteries and improving the purity of the recovered lithium salts. The process flow is simple, the operation is convenient, and the environment is friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The figure is a schematic diagram of a process for recycling lithium-ion batteries according to some embodiments. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] The embodiment of the present invention provides a method for recycling lithium-ion batteries, comprising: charging the lithium-ion battery so that the state of charge of the lithium-ion battery reaches at least 60%; disassembling the charged lithium-ion battery to separate the negative electrode sheet, the diaphragm, and the positive electrode sheet; burning the negative electrode sheet and the diaphragm, dissolving the combustion products in water, filtering, and obtaining an aqueous solution containing lithium ions and a filter residue; and separating lithium salts from the aqueous solution containing lithium ions.
[0019] According to the research and analysis of the inventors: charging the lithium-ion battery to make the state of charge of the lithium-ion battery reach at least 60% (i.e. charging to 60% SOC) can make more lithium (Li) escape from the positive electrode sheet (positive electrode material), reduce the lithium content in the positive electrode sheet (positive electrode material), and increase the lithium content in the negative electrode sheet after charging; there is a large amount of metallic lithium in the negative electrode sheet after charging, which can produce lithium oxide after combustion (sintering), and lithium oxide reacts with water to produce lithium hydroxide. Since lithium hydroxide has a high solubility in water, the product after combustion is dissolved in water, and then filtered to obtain a water-soluble lithium ion-containing lithium ion solution. Liquid, so that lithium and other components that are difficult to dissolve in water (such as copper) in the negative electrode sheet are effectively separated, which is conducive to improving the recovery rate of lithium and the purity of lithium salts. In addition, the charged lithium-ion battery is first disassembled to separate the negative electrode sheet, the diaphragm, and the positive electrode sheet, and then recycled separately, effectively avoiding the problems of great separation difficulty and poor recycling effect that are easy to occur in the process of mixing various materials (such as negative electrode sheets, diaphragms, positive electrode sheets, etc.) for recycling. In addition, the recycling method of the lithium-ion battery in the embodiment of the present invention does not need to use acid or alkali solution for the corresponding dissolution work, which is more environmentally friendly, and the process flow is simple and easy to operate. Therefore, the lithium-ion battery recycling method in the embodiment of the present invention can improve the recovery rate of lithium and the purity of the recovered lithium salt, and the process flow is simple, easy to operate, and environmentally friendly.
[0020] The schematic diagram of the process of recycling lithium ion batteries in some embodiments is as follows Figure 1 shown.
[0021] Charging the lithium-ion battery (scrapped battery) so that the state of charge of the lithium-ion battery reaches at least 60% (60% SOC) is beneficial to improving the recovery rate of lithium and improving the purity of lithium salt. The reason for this is that in the process of charging the lithium-ion battery, the state of charge (charging SOC) of the lithium-ion battery is increased, so that the lithium-ion battery forms a specific SOC battery, which can achieve more lithium from the positive electrode sheet (positive electrode material), reduce the lithium content in the positive electrode sheet (positive electrode material), and increase the lithium content in the negative electrode sheet, so that more lithium can be recovered through the recovery method of the embodiment of the present invention, which is beneficial to improving the recovery rate of lithium and improving the purity of lithium salt.
[0022] The above-mentioned process of charging the lithium-ion battery to make the state of charge of the lithium-ion battery reach at least 60% (60% SOC) may include: charging the lithium-ion battery at a rate of 1C to 60% of the nominal capacity (the specific voltage is related to the battery system, but the charging voltage cut-off scheme can be calculated based on the nominal capacity as a condition) at 25°C, and leaving it for 20 minutes.
[0023] In some embodiments, the lithium-ion battery is charged to a state of charge of at least 75% (75% SOC), further improving the recovery rate of lithium and the purity of lithium salt.
[0024] The above-mentioned process of charging the lithium-ion battery to make the state of charge of the lithium-ion battery reach at least 75% (75% SOC) may include: charging the lithium-ion battery at a rate of 1C to 75% of the nominal capacity (the specific voltage is related to the battery system, but the charging voltage cut-off scheme can be calculated based on the nominal capacity as a condition) at 25°C, and leaving it for 20 minutes.
[0025] In some embodiments, the lithium-ion battery is charged to a state of charge of at least 100% (100% SOC), further improving the recovery rate of lithium and the purity of the lithium salt.
[0026] The above-mentioned process of charging the lithium-ion battery so that the state of charge of the lithium-ion battery reaches at least 100% (100% SOC) may include: charging the lithium-ion battery at a rate of 1C to a cut-off voltage (specifically, the nominal cut-off voltage of the battery) at 25°C, and charging at a constant voltage to a cut-off current of 0.05C, and leaving it for 20 minutes.
[0027] In some embodiments, the lithium-ion battery is charged to a state of charge of at least 105% (105% SOC), further improving the recovery rate of lithium and the purity of lithium salt.
[0028] The above-mentioned process of charging the lithium-ion battery so that the state of charge of the lithium-ion battery reaches at least 105% (105% SOC) may include: charging the lithium-ion battery at a rate of 1C to a cut-off voltage + 0.1V (the above-mentioned cut-off voltage is specifically the nominal cut-off voltage of the battery) at 25°C, and charging at a constant voltage to a cut-off current of 0.05C, and leaving it for 20 minutes.
[0029] Next, the charged lithium-ion battery is disassembled to separate the negative electrode sheet, separator, and positive electrode sheet so that they can be recycled separately.
[0030] It is understandable that in the process of burning the negative electrode plate and the separator, the negative electrode plate and the separator need to be burned together, that is, the mixed material of the negative electrode plate and the separator needs to be burned.
[0031] In some embodiments, the process of burning the negative electrode plate and the separator includes: contacting the mixture of the negative electrode plate and the separator with water for combustion. This is conducive to improving the recovery rate of lithium and the purity of lithium salts. The reason for this is that after charging the lithium-ion battery to a state of charge of at least 60%, a large amount of metallic lithium exists in the negative electrode plate, which can be ignited only by contacting water, avoiding the use of other igniters for ignition, thereby avoiding the introduction of other igniters to cause pollution.
[0032] In addition, as the state of charge of the lithium-ion battery further increases, the content of metallic lithium in the negative electrode plate also increases further, and can even reach a fully charged state, making it easier to ignite (catch fire) the mixture of the negative electrode plate and the separator. That is, as the state of charge of the lithium-ion battery further increases, the difficulty of ignition (catch fire) will decrease.
[0033] In a specific implementation, water can be simply poured into the mixture of the negative electrode plate and the separator to ignite it, thereby causing the negative electrode plate and the separator to burn.
[0034] The combustion product is dissolved in water and filtered to obtain an aqueous solution containing lithium ions and a filter residue.
[0035] The process of separating the lithium salt from the aqueous solution containing lithium ions may include: subjecting the aqueous solution containing lithium ions to a dehydration treatment (such as baking dehydration) to obtain the lithium salt.
[0036] The above dehydration treatment (such as baking dehydration) can be carried out under conventional dehydration treatment conditions in the art.
[0037] In some embodiments, the lithium salt comprises lithium carbonate.
[0038] In some embodiments, the process of separating lithium salt from an aqueous solution containing lithium ions includes: introducing carbon dioxide into the aqueous solution containing lithium ions to form lithium carbonate from the lithium ions in the aqueous solution containing lithium ions, and then performing a dehydration treatment to obtain lithium salt (i.e., lithium carbonate), which is beneficial to improving the recovery rate of lithium and the purity of lithium salt. The reason for this is that the lithium in the negative electrode plate and the diaphragm is burned (sintered) to produce lithium oxide, that is, the product after combustion includes lithium oxide. In the process of dissolving the product after combustion in water, the lithium oxide reacts with water to generate lithium hydroxide, so that the aqueous solution containing lithium ions contains hydroxide and lithium ions, and due to the inevitable The aqueous solution containing lithium ions also contains a small amount of carbonate, that is, the aqueous solution containing lithium ions contains hydroxide, lithium ions, and carbonate at the same time. The lithium salt obtained by dehydrating the aqueous solution containing lithium ions includes a mixture of lithium hydroxide and lithium carbonate, that is, the purity of the lithium salt is relatively low. In the embodiment of the present invention, carbon dioxide is introduced into the aqueous solution containing lithium ions to neutralize the hydroxide, so that the aqueous solution containing lithium ions is completely converted into an aqueous solution of lithium carbonate, and then the aqueous solution containing lithium ions is dehydrated to obtain a lithium salt with higher purity, that is, lithium carbonate with higher purity, thereby further ensuring the purity of the lithium salt.
[0039] In some embodiments, the process of separating lithium salt from an aqueous solution containing lithium ions includes: introducing carbon dioxide into the aqueous solution containing lithium ions until the pH of the solution is stable, stopping the introduction of carbon dioxide, and then performing a dehydration treatment to obtain a lithium salt (i.e., lithium carbonate). The stable pH of the solution indicates that the hydroxide in the solution is fully neutralized, that is, the aqueous solution containing lithium ions is completely converted into an aqueous solution of lithium carbonate, and after dehydration treatment, a lithium salt with higher purity, i.e., lithium carbonate with higher purity, can be obtained, thereby further ensuring the purity of the lithium salt.
[0040] As mentioned above, the aqueous solution containing lithium ions is an aqueous solution containing lithium hydroxide.
[0041] In some embodiments, the process of introducing carbon dioxide into the aqueous solution containing lithium ions includes: after concentrating the aqueous solution containing lithium ions into a concentrated solution with a lithium hydroxide concentration of 15% to 22%, carbon dioxide is introduced therein. This is beneficial to improving the recovery rate of lithium and the purity of lithium salts. The reason for this is that since the solubility of lithium hydroxide is 12.8g / 100g (at 0°C, the solubility of lithium hydroxide is about 12.8g / 100g water), which is much greater than the solubility of lithium carbonate 1.3g / 100g (at 0°C, the solubility of lithium carbonate is about 1.3g / 100g water), therefore, after concentrating the aqueous solution containing lithium ions into a concentrated solution with a lithium hydroxide concentration of 15% to 22% (e.g., a saturated aqueous solution of lithium hydroxide), carbon dioxide is introduced therein to ensure that lithium carbonate is smoothly precipitated, which is beneficial to improving the recovery rate of lithium and the purity of lithium salts.
[0042] In some embodiments, the process of separating lithium salt from an aqueous solution containing lithium ions includes: concentrating the aqueous solution containing lithium ions into a concentrated solution with a lithium hydroxide concentration of 15% to 22%, and then introducing carbon dioxide into the concentrated solution until the pH of the solution stabilizes, stopping the introduction of carbon dioxide, and then performing a dehydration treatment to obtain a lithium salt.
[0043] Furthermore, after the aqueous solution containing lithium ions is concentrated into a concentrated solution with a lithium hydroxide concentration of 15% to 22% (for example, a saturated aqueous solution of lithium hydroxide), during the process of introducing carbon dioxide therein, the concentrated solution can be first filtered to obtain the precipitated lithium carbonate, and then the remaining concentrated solution can be dehydrated to obtain the remaining lithium carbonate.
[0044] The lithium-ion battery recycling method of the embodiment of the present invention also includes: kneading and screening the positive electrode plates in sequence to obtain positive electrode current collector materials and lithium-deficient positive electrode materials; and mixing the lithium-deficient positive electrode materials with lithium hydroxide and sintering them to obtain positive electrode materials. The above process can realize the recycling of the positive electrode sheet, and the recycled impurities are less and have a good recycling efficiency. The reasons are analyzed as follows: first, since the embodiment of the present invention first charges the lithium-ion battery, a large amount of lithium ions are released from the positive electrode sheet, so that the lithium content in the positive electrode material in the positive electrode sheet is significantly less than the lithium content in the positive electrode material under normal conditions. The positive electrode material in the positive electrode sheet is also a lithium-deficient positive electrode material. Secondly, the charged lithium-ion battery is disassembled, and the positive electrode sheet is separated and then rubbed, so that the lithium-deficient positive electrode material (powder) on the positive electrode collector material can fall off, thereby realizing the effective separation of the lithium-deficient positive electrode material and the positive electrode collector material. The impurity content in the lithium-deficient positive electrode material is less, which effectively avoids the problem of introducing a large amount of impurities into the recycled material during the direct crushing and recycling of conventional batteries. Thirdly, the lithium-deficient positive electrode material and lithium hydroxide are mixed and sintered, and the lithium-deficient material is supplemented with lithium to obtain the positive electrode material. Therefore, the recycling of the positive electrode sheet is realized, and the recycled impurities are less and have a good recycling efficiency.
[0045] Since some positive electrode materials have coating layers, the lithium-deficient positive electrode materials also have coating layers. If the lithium-deficient positive electrode materials with coating layers are directly subjected to lithium supplementation sintering (for example, sintering after mixing with lithium hydroxide) to obtain positive electrode materials, the coating layers will be doped into the positive electrode materials, thereby affecting the performance of the positive electrode materials. In order to avoid the above problems, the lithium-deficient positive electrode materials can be first dissolved (re-dissolved) in an acid (such as sulfuric acid), purified to obtain a solution containing different metal salts; and then separated from the solution containing different metal salts to obtain a lithium-deficient positive electrode material with higher purity.
[0046] In some embodiments, the metal in the metal salt includes one or more of nickel, cobalt, and manganese.
[0047] In some embodiments, the above-mentioned process of first dissolving (re-dissolving) the lithium-deficient positive electrode material in an acid (such as sulfuric acid) and purifying it to obtain a solution containing nickel, cobalt, and manganese; and then separating a lithium-deficient positive electrode material with higher purity from the solution containing different metal salts includes: re-dissolving the lithium-deficient positive electrode material in an acid to obtain a corresponding metal salt solution, and then adding a sodium hydroxide solution to maintain the pH at 7.6±0.1 to co-precipitate NiCo hydroxide, and then raising the pH to 8.3±0.1 to precipitate Mn hydroxide, washing the precipitate three times, re-dissolving the two hydroxides, and then co-precipitating to obtain a ternary precursor.
[0048] The purity of the metal salt in the solution containing different metal salts obtained in the embodiment of the present invention is relatively high, indicating that the lithium-ion battery recycling method of the embodiment of the present invention is also helpful to improve the recycling effect of the positive electrode material in the positive electrode sheet.
[0049] In addition, the lithium-ion battery recycling method of the embodiment of the present invention further includes: in the above-mentioned combustion process (i.e., the process of burning the negative electrode plate and the separator), a heat conversion device can be used to convert the heat generated in the combustion process into electrical energy. The electrical energy can be used to charge the lithium-ion battery so that the state of charge of the lithium-ion battery reaches at least 60%, thereby realizing energy circulation and helping to reduce the recycling cost.
[0050] Since tail gas (acid gas) is generated during the combustion of the negative electrode plate and the diaphragm, the tail gas generally includes HF, H 2 S, CO 2 To avoid exhaust gas emissions that pollute the environment, the lithium-ion battery recycling method of the embodiment of the present invention further includes: during the above combustion process, an alkaline solution may be used to absorb the exhaust gas generated during the above combustion process.
[0051] The alkaline solution may include an aqueous sodium hydroxide solution.
[0052] In some embodiments, the negative electrode current collector in the negative electrode sheet includes copper foil, and the filter residue includes the product of copper foil combustion. After washing the filter residue, a copper-containing raw material can be obtained, and the copper-containing raw material includes copper and copper oxide; and copper can be obtained by reducing the copper-containing raw material.
[0053] The present invention is described in more detail below through specific examples and comparative examples.
[0054] Example 1
[0055] This embodiment provides a method for recycling lithium-ion batteries, comprising:
[0056] Charging the lithium-ion battery so that the state of charge of the lithium-ion battery reaches 75%;
[0057] Disassemble the charged lithium-ion battery to separate the negative electrode sheet, the separator, and the positive electrode sheet;
[0058] Simply pouring water into the mixture of the negative electrode plate and the separator to ignite it, thereby burning the negative electrode plate and the separator, dissolving the combustion products in water, filtering, and obtaining an aqueous solution containing lithium ions and a filter residue;
[0059] After concentrating the aqueous solution containing lithium ions into a concentrated solution with a lithium hydroxide concentration of 15% to 22%, carbon dioxide is introduced into the concentrated solution until the pH of the solution is stable, the introduction of carbon dioxide is stopped, and then dehydration treatment is performed to obtain lithium carbonate;
[0060] The positive electrode sheet is kneaded and sieved in turn to obtain a positive electrode current collector material and a lithium-deficient positive electrode material;
[0061] The above-mentioned lithium-deficient positive electrode material is redissolved in sulfuric acid, and then sodium hydroxide solution is added to maintain the pH at 7.6±0.1 for NiCo hydroxide co-precipitation, and then the pH is increased to 8.3±0.1 to achieve Mn hydroxide precipitation. After the precipitate is washed three times, the two hydroxides are redissolved, and then co-precipitated again to purify the ternary precursor.
[0062] Example 2
[0063] This embodiment is basically the same as Embodiment 1, except that:
[0064] The lithium-ion battery is charged so that the state of charge of the lithium-ion battery reaches 100%; other conditions remain unchanged.
[0065] Example 3
[0066] This embodiment is basically the same as Embodiment 1, except that:
[0067] The lithium-ion battery is charged so that the state of charge of the lithium-ion battery reaches 105%; other conditions remain unchanged.
[0068] Example 4
[0069] This embodiment is basically the same as Embodiment 1, except that:
[0070] The lithium-ion battery is charged so that the state of charge of the lithium-ion battery reaches 60%; other conditions remain unchanged.
[0071] Example 5
[0072] This embodiment is basically the same as Embodiment 1, except that:
[0073] Replace “concentrating the aqueous solution containing lithium ions into a concentrated solution having a lithium hydroxide concentration of 15% to 22%, then introducing carbon dioxide into the solution until the pH of the solution is stable, stopping the introduction of carbon dioxide, and then dehydrating the solution to obtain lithium carbonate” with “concentrating the aqueous solution containing lithium ions into a concentrated solution having a lithium hydroxide concentration of 15% to 22%, and then introducing carbon dioxide into the solution until the pH of the solution is stable, stopping the introduction of carbon dioxide, and then dehydrating the solution to obtain lithium carbonate”; other conditions remain unchanged.
[0074] Example 6
[0075] This embodiment is basically the same as Embodiment 1, except that:
[0076] Replace “concentrating the aqueous solution containing lithium ions into a concentrated solution having a lithium hydroxide concentration of 15% to 22%, introducing carbon dioxide therein until the pH of the solution stabilizes, stopping the introduction of carbon dioxide, and then dehydrating the solution to obtain lithium carbonate” with “dehydrating the aqueous solution containing lithium ions to obtain lithium salt”; other conditions remain unchanged.
[0077] Comparative Example 1
[0078] This comparative example is basically the same as Example 1, except that:
[0079] The lithium-ion battery is not charged, so that the state of charge of the lithium-ion battery remains at 0%; other conditions remain unchanged.
[0080] Comparative Example 2
[0081] The lithium battery recycling method provided in this comparative example is carried out according to the method of Example 2 in Chinese patent document CN107196007B, and the steps are as follows:
[0082] (1) Discharge the used lithium battery by itself or immerse it in salt water until it is discharged;
[0083] (2) mechanically crushing the unpowered lithium battery obtained in step (1), adding the fragments into polycarbonate for washing, dissolving the lithium salt in the electrolyte of the unpowered lithium battery, and filtering to obtain solution A and solid A; wherein solution A is dried at 80° C. (by rotary evaporation or other common methods) to obtain the lithium salt;
[0084] (3) The solid A obtained in step (2) is crushed by a jet mill. The crushed material contains a mixture of plastic and metal, and the plastic and the metal mixture are separated; solid materials of different densities are separated according to density to obtain low-density solid materials and high-density solid materials, wherein the low-density solid materials are mainly plastics, and the high-density solid materials are metal particles and metal oxides, etc.;
[0085] (4) adding a mixed solution of excess sulfuric acid and hydrogen peroxide to the metal mixture obtained in step (3), wherein the mass fraction of hydrogen peroxide is 25%, heating and filtering to obtain solid B and solution B; the concentration of sulfuric acid is 4M, and the mass ratio of sulfuric acid to hydrogen peroxide is 7.5:2.5;
[0086] (5) adding sodium hydroxide to the solution B obtained in step (4) until the pH of the solution B is 7.5, and filtering to obtain a solid C and a solution C; the solid C is a mixture of copper hydroxide, iron hydroxide and aluminum hydroxide;
[0087] (6) adding sodium hydroxide solution to the solution C in step (5) for washing until the pH is 12, and filtering to obtain a solid D and a solution D; the solid D is a mixture of cobalt hydroxide, nickel hydroxide and manganese hydroxide;
[0088] (7) Add Na2CO3 solution to solution D in step (6) and heat to 15°C for 1 hour, and filter to obtain Li 2 CO 3 .
[0089] Comparative Example 2: 1 kg cylindrical lithium-ion battery was used as the waste battery, and NCM532 positive electrode was used to recover 37.6 g of plastic solid, 271.4 g of iron, aluminum and copper ions, 234.5 g of nickel, cobalt and manganese ions, and 150.6 g of lithium carbonate; 6 g of lithium carbonate was added to prepare the precursor.
[0090] Test example
[0091] The following parameters of each embodiment and comparative example were tested:
[0092] 1. Observe the difficulty of ignition of the mixture of the negative electrode plate and the separator (fire difficulty). The fire difficulty is divided into three levels: (1) easy: only a small amount of water is needed to ignite; (2) relatively easy, requiring open flame to ignite; (3) difficult, open flame is difficult to ignite;
[0093] 2. Purity of lithium salt: Taking lithium carbonate as an example, weigh about 0.6g of lithium carbonate sample that has been dried at 250℃-260℃ to constant mass, add 50mL of carbon dioxide-free water and 10 drops of bromocresol green-methyl red indicator solution, titrate with hydrochloric acid (c=0.5mol / L) standard titration solution until the solution changes from green to dark red, boil for 2min; after cooling, continue to titrate with hydrochloric acid standard titration solution (c=0.5mol / L) until dark red is the end point; the volume of hydrochloric acid standard titration solution added is (V1), and a blank test (V0) is performed at the same time, M=the numerical value of the molar mass of lithium carbonate, in (g / mol).
[0094] Calculate the purity of lithium carbonate W1 = {c[(V1-V0) / 1000]M / }m×100%.
[0095] The purity of lithium hydroxide is tested by referring to the purity test method of lithium carbonate.
[0096] 3. Lithium recovery rate: The lithium recovery rate is calculated based on the ratio of the lithium content in the lithium salt to the theoretical lithium content in the lithium-ion battery;
[0097] 4. Purity of metal salt: Dissolve the lithium-deficient positive electrode material, precipitate it at the corresponding pH of the metal element according to the type of metal element, then redissolve the precipitate and test the main element ratio according to the ICP main element determination scheme;
[0098] The data of the above parameters are shown in Table 1.
[0099] Table 1 Fire difficulty, type and purity of lithium salt, lithium recovery rate and purity of metal salt
[0100]
[0101] Data Analysis:
[0102] The lithium-ion battery recycling method of the embodiment of the present invention can improve the recovery rate of lithium and the purity of the recovered lithium salt, and has a simple process flow, convenient operation, and is environmentally friendly.
[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for recycling lithium-ion batteries, characterized in that: include: Charging the lithium-ion battery so that the state of charge of the lithium-ion battery reaches at least 60%; Disassemble the charged lithium-ion battery to separate the negative electrode sheet, the separator, and the positive electrode sheet; Burning the negative electrode sheet and the separator, dissolving the combustion product in water, and filtering to obtain an aqueous solution containing lithium ions and a filter residue; Lithium salt is separated from the aqueous solution containing lithium ions.
2. The recycling method according to claim 1, characterized in that: The lithium-ion battery is charged so that the state of charge of the lithium-ion battery reaches at least 75%.
3. The recycling method according to claim 2, characterized in that: The lithium ion battery is charged so that the state of charge of the lithium ion battery reaches at least 105%.
4. The recycling method according to claim 1, characterized in that: During the combustion process, an alkaline solution is used to absorb the tail gas generated during the combustion process.
5. The recycling method according to claim 1, characterized in that: The process of burning the negative electrode plate and the separator includes: contacting the mixture of the negative electrode plate and the separator with water for burning.
6. The recycling method according to claim 1, characterized in that: The lithium salt includes lithium carbonate.
7. The recycling method according to claim 6, characterized in that: The process of separating lithium salt from the aqueous solution containing lithium ions includes: introducing carbon dioxide into the aqueous solution containing lithium ions to convert lithium ions in the aqueous solution containing lithium ions into lithium carbonate, and then performing dehydration treatment to obtain the lithium salt.
8. The recycling method according to claim 7, characterized in that: The process of separating lithium salt from the aqueous solution containing lithium ions comprises: introducing carbon dioxide into the aqueous solution containing lithium ions until the pH of the solution is stable, stopping the introduction of carbon dioxide, and then performing the dehydration treatment to obtain the lithium salt.
9. The recycling method according to claim 7 or 8, characterized in that: The process of introducing the carbon dioxide into the aqueous solution containing lithium ions comprises: concentrating the aqueous solution containing lithium ions into a concentrated solution with a lithium hydroxide concentration of 15% to 22%, and then introducing carbon dioxide into the concentrated solution.
10. The recycling method according to claim 1, characterized in that: Also includes: The positive electrode sheet is kneaded and sieved in sequence to obtain a positive electrode current collector material and a lithium-deficient positive electrode material; The lithium-deficient positive electrode material and lithium hydroxide are mixed and sintered to obtain a positive electrode material.