Process method for recycling and reusing positive electrode material of waste sodium-ion battery

By converting waste Prussian blue analogs into high-specific energy sodium base oxide positive electrode material, the problem of recycling waste sodium ion batteries is solved, simple, environmentally friendly and efficient recycling and reuse is achieved, production costs are reduced, and production costs are improved. electrochemical properties.

CN119069860AInactive Publication Date: 2024-12-03WENZHOU NATECH NEW ENERGY TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411550148.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recycle and reuse waste sodium ion battery cathode materials, especially Prussian blue analogs, which have problems of environmental pollution and unused economic value.

Method used

Through complete discharge treatment, disassembly separation, drying, physical separation, mixing with metal salts and high temperature sintering, the waste Prussian blue analog is converted into a high specific energy sodium base oxide positive electrode material.

Benefits of technology

It realizes all-metal recycling with simple process, low cost and no environmental pollution, reduces the production cost of high-specific energy sodium-based layered oxide positive electrode materials, and has universality and excellent electrochemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069860A_ABST
    Figure CN119069860A_ABST
Patent Text Reader

Abstract

The invention discloses a process method for recycling a positive electrode material of a waste sodium-ion battery, which is characterized in that a metal salt is directly added into a waste Prussian blue analogue positive electrode material, and then the waste Prussian blue analogue positive electrode material is converted into a high-specific-energy layered oxide positive electrode material of the sodium-ion battery through one-step sintering. The method is simple in process and low in cost, and has good compatibility with the existing recovery technology and equipment; in the recovery process, no harmful gas is discharged, no waste residues are generated, and efficient, green and clean recovery of all metal elements is completely achieved; and the converted high-specific-energy sodium-based layered oxide positive electrode material has various components and can meet the requirements of most application scenes. Therefore, cyclic utilization of the sodium ion battery can be effectively promoted, and the method has a very wide commercial application scene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of energy material preparation and electrochemistry, and specifically relates to a process for recycling and reusing waste sodium ion battery positive electrode materials. Background Art

[0002] As a positive electrode material for sodium-ion batteries, Prussian blue analogs have the advantage of high theoretical specific capacity, which can reach 170mAh / g. In addition, Prussian blue analogs have a relatively open skeleton structure, which provides a fast channel for the insertion and extraction of sodium ions, ensuring the ion transmission efficiency during the battery charging and discharging process, thereby making the battery have better charging and discharging performance. Therefore, Prussian blue analogs are widely used in sodium-ion batteries and have become a positive electrode material system that occupies the main market share.

[0003] With the rapid growth of the new energy market, the demand for sodium-ion battery-related products is also surging. Considering capacity attenuation and safety, the average service life of sodium-ion batteries is 3-5 years. Used sodium-ion batteries with residual power or damaged structures are potential fire and explosion hazards. In addition, the final corrosion of sodium-ion batteries will also release fluorine-containing substances and heavy metals into the soil, posing a serious threat to the environment. Therefore, the recycling of used sodium-ion batteries has become a problem that needs to be solved urgently.

[0004] The recycling process of waste sodium-ion batteries based on Prussian blue analog positive electrodes also faces difficulties. First, waste sodium-ion positive electrode materials generally contain no or little precious metal elements, so the added value of recycling using traditional hydrometallurgical technology is low; secondly, the toxic cyanide in Prussian blue analogs is difficult to reuse and easily causes secondary pollution; in addition, direct landfill treatment as garbage not only increases the processing cost of waste batteries, but also causes environmental pollution. Therefore, developing a recycling process for waste sodium-ion batteries with Prussian blue analog positive electrodes that is simple in process, pollution-free, and turns waste into treasure can promote the recycling of waste sodium-ion battery positive electrode materials, maximize the economic value of waste sodium-ion battery recycling, and reduce harm to the environment. Summary of the invention

[0005] In order to solve the problems and shortcomings of the prior art, the present invention provides a process method specifically related to the recycling and reuse of waste sodium ion battery positive electrode materials, the purpose of which is to simplify the process, turn waste into treasure, realize the secondary regeneration of waste Prussian blue analog positive electrode materials into harmless recycling of high-specific energy sodium-based layered oxide positive electrode materials, and promote the sustainable development of sodium ion batteries.

[0006] A process for recycling and reusing waste sodium ion battery positive electrode materials comprises the following steps: S1: After completely discharging the waste sodium ion battery with Prussian blue analog as positive electrode material, dismantle and separate it, and the dismantling and separation requires obtaining a complete positive electrode sheet, and the positive electrode sheet is immersed in a solution for standby; S2: Take out the immersed positive electrode sheet, dry it, and then physically separate the dried positive electrode sheet to collect the aluminum foil and Prussian blue analog positive electrode material; S3: According to the content of Prussian blue analog in the recovered Prussian blue analog positive electrode material and the ratio of each transition metal element in the Prussian blue analog, calculate the mass of transition metal elements in each unit mass of the recovered positive electrode material, and then calculate the mass of transition metal / metal salt and sodium salt that needs to be added according to the composition of the layered oxide positive electrode material, grind it thoroughly, and obtain a uniformly mixed precursor; S4: Sinter the uniformly mixed precursor in a muffle furnace under a sintering atmosphere, and then sinter to a specified temperature in a one-stage heating program or a multi-stage heating program, keep it warm for a period of time, and obtain the layered oxide positive electrode material after natural cooling.

[0007] Furthermore, the waste sodium ion battery in step S1 is one or more of a waste sodium ion cylindrical battery with a Prussian blue analogue as a positive electrode material, a waste sodium ion soft-pack battery, and a waste sodium ion square battery.

[0008] Furthermore, the solution in step S1 is a mixture of any one or more of alcohol, deionized water, N-methylpolypyrrolidone, methanol, and propanol.

[0009] Furthermore, the drying method in step S2 is a mixture of one or more of air drying, vacuum drying, rake drying, spray drying and freeze drying.

[0010] Furthermore, the physical separation method in step S2 is one or more combinations of mechanical vibration separation method, ultrasonic vibration separation method and direct stripping method.

[0011] Furthermore, in step S3, the transition metal / metal salt is a mixture of one or more of transition metal / metal oxide salt, transition metal / metal chloride salt, transition metal / metal sulfate, transition metal / metal carbonate, etc.

[0012] Furthermore, in step S4, the sintering atmosphere is a protective gas, or a mixture of one or more reactive gases, the protective gas includes argon and nitrogen, and the reactive gas includes air and oxygen.

[0013] Furthermore, in the one-stage heating or multi-stage heating program in step S4, the multi-stage heating program has 2-5 stages, and the heating rate of each stage of the heating program is 1-10°C.

[0014] Furthermore, the specified temperature in step S4 is 700-1200° C., and the holding time is 5-15 h.

[0015] The present invention is beneficial in that: The process is simple and the cost is low. The recycling method provided by the present invention is to prepare a high specific energy layered oxide positive electrode material by simple disassembly, drying, separation, and then mixing with a metal salt and sintering in one step. The recycling process is simple and efficient. In the recycling process, no expensive equipment, reagents, and complex post-processing processes are involved. Only simple drying equipment, material separation equipment, and high-temperature sintering equipment are required. The cost is low and the recycling equipment in the prior art is well compatible.

[0016] Turning waste into treasure and efficient recycling. Existing recycling technologies generally selectively recycle precious metal elements in waste materials, and selectively discard non-precious metals. The recycling technology provided by the present invention belongs to full metal recycling technology, which rationally utilizes all metal elements in waste Prussian blue analog positive electrode materials and sintering to prepare high-energy-density sodium ion battery layered oxide positive electrode materials. It not only solves the recycling problem of waste Prussian blue analog positive electrode materials, but also reduces the production cost of high-energy-density sodium-based layered oxide positive electrode materials, truly turning waste into treasure and efficient recycling.

[0017] The recycling process does not pollute the environment, and no secondary waste liquid or waste gas is generated. The recycling process proposed by the present invention directly mixes the waste Prussian blue analog positive electrode material with a metal salt, fully sintering at high temperature, and completely converting it into a high-energy sodium ion battery layered oxide positive electrode material. No harmful gas is generated during the process, and no waste residue remains. At the same time, the recycling process of the present invention does not involve the solution extraction process commonly used in the prior art, so no secondary waste liquid or waste gas is generated. Therefore, the recycling process provided by the present invention is truly green, clean, and pollution-free.

[0018] The recycling of waste Prussian blue analog positive electrode materials is universal, and the high-energy-density sodium-ion battery layered oxide positive electrode materials obtained by conversion are universal. The recycling process proposed by the present invention is applicable to all types of Prussian blue analog positive electrode materials, and the full metal element recovery and conversion of waste Prussian blue analog positive electrode materials, after adding metal salts, can prepare high-energy-density sodium-ion battery layered oxide positive electrode materials for different scenarios, that is, P2, O3, P2 / O3, P2 / P3, P3 / O3, P2 / Spinel, O3 / Spinel, P2 / P3 / Spinel type high-energy-density sodium-based layered oxide positive electrode materials with different component ratios. Therefore, the high-energy-density sodium-based layered oxides obtained by recycling and conversion are universal.

[0019] The recycling process is innovative. Compared with the existing hydrometallurgical and dry metallurgical recycling processes that partially recover precious metals, the present invention innovatively directly converts waste materials into high-value-added sodium-based layered oxide positive electrode materials, and simultaneously achieves recycling and reuse. + Its unique embedding / ejection structure, excellent theoretical capacity and good conductivity make it the preferred positive electrode material for high-capacity and high-rate sodium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a process route for recycling spent Prussian blue analog sodium-ion batteries.

[0021] Figure 2 This is a scanning electron microscope (SEM) photograph of a waste Prussian blue analog.

[0022] Figure 3 The Na prepared by converting waste Prussian blue analogues in Example 1 0.85 Mn 0.85 Fe 0.1 Ti 0.05 Scanning electron microscope (SEM) image of O2 layered oxide cathode material.

[0023] Figure 4 This is the X-ray diffraction pattern (XRD) of the layered oxide positive electrode material prepared using waste Prussian blue analogues in Example 1.

[0024] Figure 5 This is the first cycle charge and discharge curve of the layered oxide positive electrode material prepared using waste Prussian blue analogues in Example 1 at a current density of 0.1 C in the voltage range of 2-4 V.

[0025] Figure 6 The rate performance of the layered oxide positive electrode material prepared using waste Prussian blue analogues in Example 1 in the voltage range of 2-4 V.

[0026] Figure 7 The long cycle performance of the layered oxide positive electrode material prepared using waste Prussian blue analogues in Example 1 at a current density of 1 C in the voltage range of 2-4 V.

[0027] Figure 8 The charge and discharge curves of the layered oxide positive electrode material prepared using waste Prussian blue analogues in Example 1 at a current density of 0.1 C in the voltage range of 2-4.3 V.

[0028] Fig. 9 The rate performance of the layered oxide positive electrode material prepared using waste Prussian blue analogues in Example 1 in the voltage range of 2-4.3 V.

[0029] Fig.10 This is the long cycle performance of the layered oxide positive electrode material prepared using waste Prussian blue analogues in Example 1 at a current density of 1 C in the voltage range of 2-4.3 V.

[0030] Fig.11 The Na prepared from waste Prussian blue analogue in Example 2 0.9 Cu 0.22 Mg 0.11 Fe 0.33 Mn 0.34 Scanning electron microscope (SEM) image of O2 layered oxide cathode material.

[0031] Fig.12 This is the X-ray diffraction pattern (XRD) of the material in Example 2.

[0032] Fig.13 The charge and discharge curves of the material in Example 2 at a voltage range of 2-4 V and a current density of 0.1 C.

[0033] Fig.14 It is the rate performance of the material in Example 2 in the voltage range of 2-4 V.

[0034] Fig.15 This is the long cycle performance of the material in Example 2 at a voltage range of 2-4 V and a current density of 1 C.

[0035] Fig.16 This is the first cycle charge and discharge curve of the material in Example 2 at a voltage range of 2-4.3 V and a current density of 0.1 C.

[0036] Fig.17 It is the rate performance of the material in Example 2 in the voltage range of 2-4.3 V.

[0037] Fig.18 This is the long cycle performance of the material in Example 2 in the voltage range of 2-4.3 V and a current density of 1 C.

[0038] Fig.19 The Na prepared from waste Prussian blue analogue in Example 3 0.9 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 Scanning electron microscope (SEM) image of O2 layered oxide cathode material.

[0039] Fig. 20 This is the X-ray diffraction pattern (XRD) of the material in Example 3.

[0040] Fig.21This is the first cycle charge and discharge curve of the material in Example 3 at a voltage range of 2-4 V and a current density of 0.1 C.

[0041] Fig. 22 It is the rate performance of the material in Example 3 in the voltage range of 2-4 V.

[0042] Fig.23 The Na prepared from waste Prussian blue analogues in Example 4 0.9 Ni 2 / 9 Mg 1 / 9 Fe 1 / 3 Mn 1 / 3 Scanning electron microscope (SEM) image of O2 layered oxide cathode material.

[0043] Fig.24 This is the X-ray diffraction pattern (XRD) of the material in Example 4.

[0044] Fig.25 This is the first cycle charge and discharge curve of the material in Example 4 at a voltage range of 2-4 V and a current density of 0.1 C.

[0045] Fig.26 It is the rate performance of the material in Example 4 in the voltage range of 2-4 V.

[0046] Fig. 27 The long cycle performance of the material in Example 4 in the voltage range of 2-4 V and a current density of 1 C.

[0047] Fig.28 This is the first cycle charge and discharge curve of the material in Example 4 at a voltage range of 2-4.3 V and a current density of 0.1 C.

[0048] Fig.29 It is the rate performance of the material in Example 4 in the voltage range of 2-4.3 V.

[0049] Fig.30 This is the long cycle performance of the material in Example 4 in the voltage range of 2-4.3 V and a current density of 1 C. DETAILED DESCRIPTION

[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The test methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials can be obtained from commercial channels unless otherwise specified.

[0051] Embodiment 1: Na 0.85 Mn 0.85 Fe 0.1Ti 0.05 Preparation of O2 high specific energy sodium-based layered oxide positive electrode material; S1: After the waste sodium ion battery with Fe / Mn-based Prussian blue analog as positive electrode material is completely discharged, it is disassembled and separated. The disassembly and separation requires obtaining complete positive electrode and negative electrode sheets. And the positive electrode sheets, diaphragms, negative electrode sheets, shells, etc. are sorted and collected. Then the positive electrode sheets are soaked in an alcohol solution with a concentration of 95-100% to remove the residual sodium and electrolyte on the surface of the electrode sheets for standby use. S2: Take out the soaked positive electrode sheets and dry them at 100-120 ℃ in a blast drying oven for 3-10 h, then manually peel off the dried positive electrode sheets to collect aluminum foil and waste Prussian blue analog positive electrode materials. S3: According to the content of Prussian blue analog in the recycled positive electrode material and the ratio of Fe and Mn elements in the Prussian blue analog, calculate the mass of transition metal elements in each gram of recycled positive electrode material. Then, according to the composition of the layered oxide positive electrode material, the mass of transition metal / metal salt and sodium salt to be added is calculated, and 0.2715 g of waste Prussian blue analogue, 1.2894 g of transition metal oxide Mn2O3, 0.0799 g of transition metal salt TiO2 and 0.9459 g of sodium salt Na2CO3 are taken, fully ground, mixed evenly and set aside. S4: In an air atmosphere, a porcelain boat containing a uniformly mixed precursor is sintered in a muffle furnace. The oxygen in the air can ensure that the material is fully oxidized during the conversion process. Then, it is heated to 950-1100 ℃ at a heating rate of 3-10 ℃ / min and kept warm for 6-12h. After natural cooling, a high specific energy layered oxide positive electrode material is obtained.

[0052] 2. Na 0.85 Mn 0.85 Fe 0.1 Ti 0.05 Assembly of O2 sodium-ion batteries The ratio is Na 0.85 Mn 0.85 Fe 0.1 Ti 0.05The layered oxide of O2 is a positive electrode material with excellent electrochemical performance obtained by our research group during the experimental exploration process, and has good application prospects. According to the current empirical ratio of sodium ion battery slurry preparation, the prepared positive electrode material, conductive carbon black (conductive agent) and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 70:20:10, and a certain proportion of pure N-methylpolypyrrolidone (NMP) is added as a solvent. The oscillator is oscillated at a frequency of 10-300 times / second, each time for 3-5 minutes, and a uniform slurry is obtained after oscillating 5-10 times. Then the slurry is evenly coated on an aluminum foil with a thickness of 10-20 μm, and the slurry coating thickness is 150-300 μm. Then the electrode piece is transferred to a vacuum drying oven and dried at 100-120℃ for 5-12 hours, and then the cut piece is taken out. The diameter of the cut electrode piece is 1-1.5 cm, which is used as a positive electrode piece for standby. In an inert gas-protected glove box, the positive electrode sheet, separator and sodium sheet were assembled into a button cell, 60-150 μL of commercial electrolyte was added and then packaged. The assembled battery was left to stand for 2-10 h before electrochemical testing. Figure 1 As shown in the figure, it is a flow chart of the entire recycling and reuse of waste Prussian blue analog positive electrode materials and their conversion into high specific energy sodium ion battery layered oxide positive electrode materials. Figure 2 As shown by scanning electron microscopy (SEM), the spent Prussian blue analogs recovered from spent sodium-ion batteries still maintain a cubic morphology and are bonded together with binders, conductive carbon black, etc. Figure 3 SEM showed that the Na 0.85 Mn 0.85 Fe 0.1 Ti 0.05 O2 material shows a typical lamellar structure of layered oxides. Figure 4 The powder X-ray diffraction (XRD) test results show that the Na synthesized in Example 1 0.85 Mn 0.85 Fe 0.1 Ti 0.05 O2 material is a P2 / O3 composite layered oxide positive electrode material. Figure 5 The charge-discharge curves of the material at 2-4 V show that the Na 0.85 Mn 0.85 Fe 0.1 Ti 0.05 The specific capacity of the O2 material at a current density of 0.1 C is 145.3 mAh g -1 , showing high capacity characteristics. Figure 6 The specific energy diagram of the material at 2-4 V with voltage shows that the specific energy of the material synthesized in Example 1 at 2-4 V is 397.2 Wh kg -1, showing high specific energy characteristics. Figure 7 The rate performance of the material at 2-4 V shows that the material synthesized in Example 1 still exhibits 79.9 mAh g at 2 C. -1 The specific capacity at 0.1 C is 81.4%, showing excellent rate performance. Figure 8 The long cycle performance of the material at 2-4 V shows that the specific capacity of the material synthesized in Example 1 at a current density of 1 C is 95.5 mAh g -1 , and after 100 cycles, the capacity retention rate is 78.9%, showing good long-cycle stability. Fig. 9 The charge-discharge curves of the material at 2-4.3 V show that the specific capacity of the material synthesized in Example 1 at a current density of 0.1 C is 153.3 mAh g -1 , showing high specific capacity characteristics. Fig.10 The specific energy diagram of the material in Example 1 at 2-4.3 V with voltage variation shows that the specific energy of the material synthesized in Example 1 at 2-4.3 V is 424.2 Wh kg -1 , showing high specific energy characteristics. Fig.11 The rate performance of the material at 2-4.3 V shows that the material synthesized in Example 1 still exhibits a capacity of 77.3 mAh g at 2 C. -1 The specific capacity shows excellent high rate performance. Fig.12 The long cycle of the material in Example 1 at 2-4.3 V shows that the specific capacity of the material in Example 1 at 1 C current density is 87.7 mAh g -1 , and after 100 cycles, the capacity retention rate was 74.6%, showing good long-cycle stability. Analysis of the experimental results shows that Na 0.85 Mn 0.85 Fe 0.1 Ti 0.05 O2 layered oxide positive electrode material, which exhibits high specific capacity and excellent rate performance and long cycle performance, proving that it has good electrochemical performance. Therefore, waste Prussian blue analogs can be used as raw materials to prepare high specific energy layered oxide positive electrode materials, and this invention has great commercial application prospects.

[0053] Embodiment 2: 1. Na 0.9 Cu 0.22 Mg 0.11 Fe 0.33 Mn 0.34Preparation of O2 layered oxide positive electrode material; S1: After the waste sodium ion battery with Fe / Mn-based Prussian blue analog positive electrode material is completely discharged, it is disassembled and separated. The disassembly and separation requires obtaining complete positive electrode sheets and negative electrode sheets. And the positive electrode sheets, diaphragms, negative electrode sheets, shells, etc. are sorted and collected. Then the positive electrode sheets are soaked in an alcohol solution with a concentration of 95-100% to remove the residual sodium and electrolyte on the surface of the electrode sheets for standby use. S2: Take out the soaked positive electrode sheets and dry them in a blast drying oven at 100-120 ℃ for 3-10 h, then manually peel off the dried positive electrode sheets to collect aluminum foil and waste Prussian blue analog positive electrode materials. S3: According to the content of Prussian blue analogs in the recycled positive electrode materials and the ratio of Fe and Mn elements in the Prussian blue analogs, calculate the mass of transition metal elements Fe and Mn per gram of recycled positive electrode materials. Then, according to the composition of the layered oxide positive electrode material, the mass of transition metal / metal salt and sodium salt to be added is calculated, and 0.9049 g of waste Prussian blue analog positive electrode material, 0.8749 g of transition metal salt Mn2O3, 0.3319 g of transition metal salt CuO, 0.0896 g of metal salt MgO and 1.0016 g of sodium salt Na2CO3 are taken, fully ground, mixed evenly and set aside. S4: In an air atmosphere, a porcelain boat containing a uniformly mixed precursor is sintered in a muffle furnace. The oxygen in the air can ensure that the material is fully oxidized during the conversion process. Then, it is heated to 950-1100 ℃ at a heating rate of 3-10 ℃ / min and kept warm for 6-12h. After natural cooling, a high specific energy layered oxide positive electrode material is obtained.

[0054] 2. Na 0.9 Cu 0.22 Mg 0.11 Fe 0.33 Mn 0.34 Assembly of O2 sodium-ion batteries Composition: Na 0.9 Cu 0.22 Mg 0.11 Fe 0.33 Mn 0.34The layered oxide of O2 is a positive electrode material with excellent electrochemical performance obtained by our research group during the experimental exploration process, and has good application prospects. According to the current empirical ratio of sodium ion battery slurry preparation, the prepared positive electrode material, conductive carbon black (conductive agent) and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 70:20:10, and a certain proportion of pure N-methylpolypyrrolidone (NMP) is added as a solvent. The oscillator is oscillated at a frequency of 10-300 times / second for 3-5 minutes each time, and a uniform slurry is obtained after oscillating 5-10 times. Then the slurry is evenly coated on an aluminum foil with a thickness of 10-20 μm, and the slurry coating thickness is 150-300 μm. Then the electrode piece is transferred to a vacuum drying oven at 100-120 ℃ and dried for 5-12 hours, and then the cut piece is taken out. The diameter of the cut electrode piece is 1-1.5 cm, which is used as a positive electrode piece for standby use. In an inert gas-protected glove box, the positive electrode, separator and sodium sheet were assembled into a button cell, 60-150 μL of commercial electrolyte was added and then packaged. The assembled battery was left to stand for 2-10 h before the electrochemical performance test. Fig.13 As shown in the SEM in Example 2, Na 0.9 Cu 0.22 Mg 0.11 Fe 0.33 Mn 0.34 O2 material shows a typical lamellar structure of layered oxides, with a particle size distribution between 2-5 μm. Fig.14 The energy spectrum (EDS) of the material shows that the elements in the material synthesized in Example 2 are uniformly distributed. Fig.15 The XRD test results show that the material synthesized in Example 2 is an O3-type layered oxide positive electrode material. Fig.16 The charge-discharge curve of the material at 2-4 V shows that the specific capacity of the cathode material synthesized in Example 2 at a current density of 0.1 C is 107.1 mAh g -1 , showing high specific capacity characteristics. Fig.17 The specific energy diagram of the material at 2-4 V with voltage shows that the specific energy of the material synthesized in Example 2 at 2-4 V is 326.9 Wh kg -1 , showing high specific energy characteristics. Fig.18 The rate performance of the material in Example 2 at 2-4 V shows that the material in Example 2 still exhibits a capacity of 70.9 mAh g at 2 C. -1 The specific capacity shows excellent rate performance. Fig.19 The long cycle of the material at 2-4 V shows that the specific capacity of the material in Example 2 at 1 C current density is 83.8 mAh g -1 , and after 200 cycles, the capacity retention rate is 81.3%, showing excellent long-cycle stability. Fig. 20 The charge-discharge curves of the material at 2-4.3 V show that the specific capacity of the cathode material synthesized in Example 2 at a current density of 0.1 C is 147.6 mAh g -1 , showing high specific capacity characteristics. Fig.21 The specific energy diagram of the material in Example 2 at 2-4.3 V with voltage variation shows that the specific energy of the material synthesized in Example 2 at 2-4.3 V is 475.9 Whkg -1 , showing high specific energy characteristics. Fig. 22 The rate performance of the material in Example 2 at 2-4.3 V shows that the material in Example 2 still exhibits 100.8 mAh g at 2 C. -1 The specific capacity shows excellent high rate performance. Fig.23 The long cycle of the material at 2-4.3 V shows that the specific capacity of the cathode material in Example 2 at 1 C current density is 113.6 mAh g -1 , and after 100 cycles, the capacity retention rate was 72.8%, showing excellent long-cycle stability. Analysis of the experimental results shows that Na 0.9 Cu 0.22 Mg 0.11 Fe 0.33 Mn 0.34 O2 layered oxide positive electrode material, which exhibits excellent rate performance and outstanding long cycle performance, proving that it has good electrochemical performance. Therefore, the preparation of high-capacity layered oxide positive electrode materials using waste Prussian blue analogs as raw materials is universal, and this invention has important reference value for the recycling and reuse of waste Prussian blue analogs.

[0055] Embodiment 3: 1. Na 0.9 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 Preparation of O2 layered oxide cathode materials; S1: After the waste sodium ion battery with Ni / Fe / Mn-based Prussian blue analog as the positive electrode material is completely discharged, it is disassembled and separated. The disassembly and separation requires obtaining complete positive and negative electrode sheets. And the positive electrode sheets, diaphragms, negative electrode sheets, shells, etc. are sorted and collected. Then the positive electrode sheets are soaked in an alcohol solution with a concentration of 95-100% to remove the residual sodium and electrolyte on the surface of the electrode sheets for standby use. S2: Take out the soaked positive electrode sheets, dry them at 100-120 ℃ in a blast drying oven for 3-10 h, and then manually peel off the dried positive electrode sheets to collect aluminum foil and waste Prussian blue analog positive electrode materials. S3: According to the content of Prussian blue analogs in the recycled positive electrode materials and the ratio of Ni, Fe and Mn elements in the Prussian blue analogs, calculate the mass of transition metal elements Ni, Fe and Mn per gram of recycled positive electrode materials. Then, according to the composition of the layered oxide positive electrode material, the mass of transition metal / metal salt and sodium salt that needs to be added is calculated. Take 1 g of waste Prussian blue analog positive electrode material, 0.5815 g of transition metal salt Mn2O3, 0.5503 g of transition metal salt NiO, and 1.0541 g of sodium salt Na2CO3, grind them thoroughly, mix them evenly, and set them aside. S4: In an air atmosphere, sinter a porcelain boat containing a uniformly mixed precursor in a muffle furnace. The oxygen in the air can ensure that the material is fully oxidized during the conversion process. Then, heat to 950-1100 ℃ at a heating rate of 3-10 ℃ / min and keep warm for 6-12h. After natural cooling, a high specific energy layered oxide positive electrode material is obtained.

[0056] 2. Na 0.9 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 Assembly of O2 sodium-ion batteries Composition: Na 0.9 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3The layered oxide of O2 is a layered oxide positive electrode material with excellent electrochemical properties that is recognized in the current research field of sodium ion battery positive electrode materials. According to the current empirical ratio of sodium ion battery slurry preparation, the prepared positive electrode material, conductive carbon black (conductive agent) and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 70:20:10, and a certain proportion of pure N-methylpolypyrrolidone (NMP) is added as a solvent. The oscillator is oscillated at a frequency of 10-300 times / second for 3-5 minutes each time, and a uniform slurry is obtained after oscillating 5-10 times. Then the slurry is evenly coated on an aluminum foil with a thickness of 10-20 μm, and the slurry coating thickness is 150-300 μm. Then the pole piece is transferred to a vacuum drying oven and dried at 100-120 ° C for 5-12 h, and then the cut piece is taken out. The diameter of the cut pole piece is 1-1.5 cm, which is used as a positive pole piece for standby. In an inert gas-protected glove box, the positive electrode sheet, separator and sodium sheet were assembled into a button battery, and 60-150 μL of commercial electrolyte was added and then packaged. The assembled battery was left to stand for 2-10 h before the electrochemical performance test. Fig.24 SEM shows that the Na 0.9 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 material shows a typical lamellar structure of layered oxides. Fig.25 The energy spectrum (EDS) in the embodiment 3 shows that the Na, Ni, Fe, Mn and O elements are evenly distributed in the positive electrode material, indicating that no element enrichment occurs during the conversion process. Fig.26 The XRD test results show that the material prepared in Example 3 is an O3-type layered oxide positive electrode material. Fig. 27 The first cycle charge-discharge curve of the material at 2-4 V shows that the specific capacity of the cathode material synthesized in Example 3 at a current density of 0.1 C is 109.1 mAh g -1 , showing high specific capacity characteristics. Fig.28 The specific energy diagram of the material at 2-4 V shows that the specific energy of the material synthesized in Example 3 at 0.1 C is 338.6 Wh kg -1 , showing high specific energy characteristics. Fig.29 The rate performance of the material at 2-4 V shows that the material synthesized in Example 3 still exhibits 71.3 mAh g at 2 C. -1 The specific capacity of Prussian blue can be successfully synthesized using recycled Prussian blue analogs. 0.9 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3O2 layered oxide positive electrode material, which exhibits high specific capacity characteristics and fast charging characteristics under high current density. Therefore, waste Prussian blue analogs can be directly converted into high specific capacity layered oxide positive electrode materials as raw materials. This invention has important reference value for the recycling and reuse of waste Prussian blue analogs.

[0057] Embodiment 4: 1. Na 0.9 Ni 2 / 9 Mg 1 / 9 Fe 1 / 3 Mn 1 / 3 Preparation of O2 layered oxide cathode materials S1: After the waste sodium ion battery with Ni / Fe / Mn-based Prussian blue analog positive electrode material is completely discharged, it is disassembled and separated. The disassembly and separation requires obtaining complete positive and negative electrode sheets. And the positive electrode sheets, diaphragms, negative electrode sheets, shells, etc. are sorted and collected. Then the positive electrode sheets are soaked in an alcohol solution with a concentration of 95-100% to remove the residual sodium and electrolyte on the surface of the electrode sheets for standby use. S2: Take out the soaked positive electrode sheets, dry them in a blast drying oven at 100-120 ℃ for 3-10 h, and then manually peel off the dried positive electrode sheets to collect aluminum foil and waste Prussian blue analog positive electrode materials. S3: According to the content of Prussian blue analogs in the recycled positive electrode materials and the ratio of Ni, Fe and Mn elements in the Prussian blue analogs, calculate the mass of transition metal elements Ni, Fe and Mn per gram of recycled positive electrode materials. Then, according to the composition of the layered oxide positive electrode material, the mass of transition metal / metal salt and sodium salt to be added is calculated. 1 g of waste Prussian blue analog positive electrode material, 0.5815 g of transition metal salt Mn2O3, 0.5503 g of transition metal salt NiO, 0.1491 g of metal salt MgO, 1.0541 g of sodium salt Na2CO3 are taken, fully ground, mixed evenly, and set aside. S4: In an air atmosphere, a porcelain boat containing a uniformly mixed precursor is sintered in a muffle furnace. The oxygen in the air can ensure that the material is fully oxidized during the conversion process. Then, it is heated to 950-1100 ℃ at a heating rate of 3-10 ℃ / min and kept warm for 6-12h. After natural cooling, a high specific energy layered oxide positive electrode material is obtained.

[0058] 2. Na 0.9 Ni 2 / 9 Mg 1 / 9 Fe 1 / 3 Mn 1 / 3 Assembly of O2 sodium-ion batteries Composition: Na 0.9 Ni 2 / 9 Mg 1 / 9 Fe 1 / 3 Mn 1 / 3The layered oxide of O2 is a classic layered oxide positive electrode material in the field of sodium ion battery positive electrode material research. 0.9 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is used to replace the Mg element for modification. According to the current empirical ratio for the preparation of sodium ion battery slurry, the prepared positive electrode material, conductive carbon black (conductive agent) and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 70:20:10, and a certain proportion of pure N-methylpolypyrrolidone (NMP) is added as a solvent. The oscillator is oscillated at a frequency of 10-300 times / second for 3-5 minutes each time, and a uniform slurry is obtained after oscillating 5-10 times. The slurry is then evenly coated on an aluminum foil with a thickness of 10-20 μm, and the slurry coating thickness is 150-300 μm. The pole piece is then transferred to a vacuum drying oven and dried at 100-120 °C for 5-12 hours, and then the cut piece is taken out. The diameter of the cut pole piece is 1-1.5 cm, which is used as a positive pole piece for standby use. In an inert gas-protected glove box, the positive electrode sheet, separator and sodium sheet were assembled into a button battery, and 60-150 μL of commercial electrolyte was added and then packaged. The assembled battery was left to stand for 2-10 h before electrochemical testing. Fig.30 As shown in the SEM, the Na synthesized from waste Prussian blue analogs in Example 4 0.9 Ni 2 / 9 Mg 1 / 9 Fe 1 / 3 Mn 1 / 3 O2 materials, showing a large typical lamellar structure. The Na 0.9 Ni 2 / 9 Mg 1 / 9 Fe 1 / 3 Mn 1 / 3 O2 layered oxide positive electrode material, which exhibits high energy density characteristics and fast charging characteristics under high current density. Therefore, it is proved again that waste Prussian blue analogs can be directly converted into high-performance layered oxide positive electrode materials, indicating that the recycling and conversion process is universal for the recycled materials. This invention provides a new idea for the recycling and reuse of waste Prussian blue analogs.

[0059]

[0060] The process provided by the present invention uses waste Prussian blue analogs as precursors, adds appropriate amounts of transition metal salts, metal salts and sodium salts according to the ratio, and follows the sintering procedure described in the invention to prepare high specific energy layered oxide positive electrode materials of different crystal types and different components. Table 1 shows the crystal types, component compositions and 0.1 C specific capacities of high specific energy layered oxide positive electrode materials that can be prepared. The layered oxide positive electrode materials that can be prepared by the present invention are not limited to the positive electrode materials listed in this table. Any layered oxide positive electrode materials other than those listed in Table 1 that are prepared by simply modifying the method described in the present invention still belong to the technical solution of the present invention.

[0061] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A process for recycling and reusing the positive electrode material of waste sodium ion batteries, characterized in that: The following steps are involved: S1: After completely discharging the waste sodium-ion batteries using Prussian blue analogs as positive electrode materials, they are disassembled and separated. The disassembly and separation requires obtaining complete positive electrode sheets, which are then immersed in a solution for standby use; S2: Taking out the immersed positive electrode sheets, drying them, and then physically separating the dried positive electrode sheets to obtain aluminum foil and Prussian blue analog positive electrode materials; S3: Calculating the mass of transition metal elements per unit mass of the recovered positive electrode materials based on the content of Prussian blue analogs in the recovered Prussian blue positive electrode materials and the ratio of each transition metal element in the Prussian blue analogs, and then calculating the mass of transition metals / metal salts and sodium salts that need to be additionally added based on the components of the layered oxide positive electrode materials, and grinding them fully to obtain a uniformly mixed precursor; S4: Sinter the uniformly mixed precursor in a muffle furnace under a sintering atmosphere, then sinter to a specified temperature using a one-stage heating program or a multi-stage heating program, keep the temperature for a period of time, and obtain a layered oxide positive electrode material after natural cooling.

2. The process for recycling and reusing the positive electrode material of waste sodium ion batteries according to claim 1, characterized in that: The waste sodium ion battery in step S1 is one or more of a waste sodium ion cylindrical battery using a Prussian blue analog as a positive electrode material, a waste sodium ion soft-pack battery, and a waste sodium ion square battery.

3. The process for recycling and reusing the positive electrode material of waste sodium ion batteries according to claim 1, characterized in that: The solution in step S1 is a mixture of any one or more of alcohol, deionized water, N-methylpolypyrrolidone, methanol, and propanol.

4. The process for recycling and reusing the positive electrode material of waste sodium ion batteries according to claim 1, characterized in that: The drying method in step S2 is a mixture of one or more of air drying, vacuum drying, rake drying, spray drying and freeze drying.

5. The process for recycling and reusing the positive electrode material of waste sodium ion batteries according to claim 1, characterized in that: The physical separation method in step S2 is one or more combinations of mechanical vibration separation, ultrasonic vibration separation and direct stripping.

6. The process for recycling and reusing the positive electrode material of waste sodium ion batteries according to claim 1, characterized in that: In step S3, the transition metal / metal salt is a mixture of one or more of transition metal / metal oxide salt, transition metal / metal chloride salt, transition metal / metal sulfate, and transition metal / metal carbonate.

7. The process for recycling and reusing the positive electrode material of waste sodium ion batteries according to claim 1, characterized in that: In step S4, the sintering atmosphere is a protective gas, or a mixture of one or more reactive gases. The protective gas includes argon and nitrogen, and the reactive gas includes air and oxygen.

8. The process for recycling and reusing the positive electrode material of waste sodium ion batteries according to claim 1, characterized in that: In step S4, the one-stage or multi-stage heating program has 2-5 stages, and the heating rate of each stage is 1-10°C.

9. The process for recycling and reusing the positive electrode material of waste sodium ion batteries according to claim 1, characterized in that: In step S4, the sintering temperature is 700-1200°C and the holding time is 5-15 h.

Citation Information

Patent Citations

  • Method for preparing cathode material of lithium ion battery

    CN103956533A

  • Layered oxide positive electrode material of lithium as well as preparation and application of layered oxide positive electrode material

    CN112978808A

  • Sodium ion battery Prussian sodium positive electrode material recovery method and application thereof

    CN117638279A

  • Universal method for ultrafast preparation of sodium ion battery layered oxide positive electrode material based on Prussian blue analogue and application

    CN117747797A

  • Recycling method and application of waste sodium-ion battery positive electrode material

    CN118231824A