Arbitrary-layer interconnected high-density circuit board and preparation process thereof

Through the room temperature pressing process of modified silver powder, conductive adhesives and modified nanoboronitride powder, the problems of high-temperature pressing and excessive plate body in the existing technology are solved, and light and high density are achieved and long-lived interconnected circuit boards.

CN119072031AActive Publication Date: 2024-12-03江西志博信科技股份有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411072398.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-12-03
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing high-density circuit boards of any layer interconnected high-density circuit boards take a long time and cause the plate body to be too large, which cannot meet the thin and compact needs of electronic products.

Method used

Using modified silver powder and conductive adhesive, modified nanoboronitride powder and activated alumina, etc., light and thin, any layer interconnected high-density circuit board is prepared through a normal temperature pressing process, and the advantages of conductive adhesive and insulating coatings are used. Performance improves the conductivity and insulation performance of circuit boards.

Benefits of technology

It realizes the thinness and compactness of the circuit board, improves the conductivity and insulation performance, extends the service life of the circuit board, and reduces the preparation time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072031A_ABST
    Figure CN119072031A_ABST
Patent Text Reader

Abstract

The invention provides an arbitrary-layer interconnected high-density circuit board and a preparation process thereof, and belongs to the technical field of printed circuit boards. The preparation process comprises the following steps: modifying the silver powder and preparing the conductive adhesive; carrying out surface pretreatment on nano boron nitride powder and modifying by using dopamine hydrochloride; activating the aluminum oxide by gamma-glycidyl ether oxypropyl trimethoxy silane; adding phenyltriethoxysilane to prepare a modifier, and then preparing an insulating coating; and preparing a substrate and laminating the substrate at normal temperature. According to the invention, the two copper foils and the insulating coating are compounded to prepare the PCB substrate, the PCB substrate is bonded by the conductive adhesive, and the PCB substrate and the conductive adhesive are laminated at one time at normal temperature to form the high-density circuit board with the interconnected layers, so that compared with a traditional circuit board obtained by laminating prepregs and copper foils layer by layer at high temperature, the high-density circuit board has the advantages of being lighter and thinner, and meanwhile, the circuit board is more convenient to manufacture. The insulating paint has good insulating performance and the conductive adhesive has good conductivity, so that the manufactured high-density circuit board with any layer interconnection can work normally.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printed circuit boards, and in particular to a high-density circuit board with arbitrary layer interconnection and a preparation process thereof. Background Art

[0002] High-density interconnection circuit board is a circuit board with a higher line distribution density made by micro blind buried via technology. It can achieve higher wiring density and more complex circuit design in a smaller size, and arbitrary layer interconnection is a more complex electrical connection design of high-density interconnection circuit board.

[0003] At present, the existing arbitrary-layer interconnected high-density circuit boards include substrates and single-sided boards. The single-sided boards are laminated on the substrates through semi-cured layers. Since the semi-cured layers need to be heated at high temperatures for a certain period of time to form stable semi-cured layers, the high-density interconnected circuit boards need to be laminated layer by layer for multiple times. This process consumes a lot of time. Moreover, the semi-cured layers composed of resin and reinforcing materials are usually thicker. If the high-density interconnected circuit boards have more layers, they will be too large and not light, thin and compact enough to meet the needs of electronic products.

[0004] Therefore, we proposed a high-density circuit board with arbitrary layer interconnection that has a short pressing time and is thinner and lighter, and its preparation process to meet the needs of electronic products. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention aims to provide a high-density circuit board with arbitrary layer interconnection and a preparation process thereof.

[0006] S1: Modification of silver powder and preparation of conductive adhesive Adding γ-glycidyloxypropyltrimethoxysilane to flaky silver powder and spherical silver powder to prepare modified silver powder, then using butyl acrylate, methyl methacrylate, 2-ethylhexyl acrylate and lauryl acrylate as raw materials to prepare an intermediate, and then adding the modified silver powder to the intermediate to obtain a conductive adhesive; S2: Surface pretreatment of nano-boron nitride powder and modification with dopamine hydrochloride The nano boron nitride powder and the sodium hydroxide solution are heated and stirred to pre-treat the surface of the nano boron nitride powder, and then the nano boron nitride powder is uniformly mixed with the mixed solution, and dopamine hydrochloride is added for modification to obtain modified nano boron nitride; S3: γ-glycidyloxypropyltrimethoxysilane activated alumina Dissolve γ-glycidyloxypropyltrimethoxysilane in ethanol, add acetic acid until the pH is adjusted to 3-4, then add alumina, heat reflux at 60-70° C. and stir for 5-6 hours, cool naturally to room temperature, filter, wash with ethanol and dry to obtain activated alumina; S4: Add phenyltriethoxysilane to prepare a modifier and then prepare an insulating coating Anhydrous ethanol, anhydrous methanol, hydrochloric acid, deionized water, phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane are mixed to prepare a modifier, which is then mixed with epoxy resin, diaminodiphenylmethane, the modified nano boron nitride and the modified alumina to obtain an insulating coating; S5: Prepare substrate and press the substrate at room temperature The above-mentioned insulating coating is coated on the upper surface of the copper foil, and then another copper foil is attached to form a PCB substrate. After the PCB substrate is laser drilled and filled with copper by electroplating, it is bonded with the above-mentioned conductive adhesive and pressed at room temperature to obtain a high-density circuit board with arbitrary layer interconnections.

[0007] Furthermore, the modified silver powder and the preparation of the conductive adhesive in step S1 specifically include the following steps: S1.1: Add flaky silver powder and spherical silver powder into a planetary centrifugal mixer at a mass ratio of 3-5:6-8, then add anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane accounting for 3-5% of the total mass of flaky silver powder and spherical silver powder at a solid-liquid ratio of 1g:10-12mL, stir and mix evenly, then place in an oven and dry at 60-80°C for 2-3h to obtain modified silver powder; S1.2: Add butyl acrylate, methyl methacrylate, 2-ethylhexyl acrylate and lauryl acrylate into a mixing tank, then add γ-methacryloxypropyltrimethoxysilane and ethyl acetate into the mixing tank, stir and mix thoroughly to obtain a premixed solution; S1.3: nitrogen is introduced into the reactor until all the air is exhausted, and then 2 / 3 of the premixed liquid is added into the reactor, and heated at 70-80°C for 30-40 min, while stirring at a rate of 300-400 r / min; S1.4: Adjust the stirring rate to 100-200 r / min, add the remaining premix, β-hydroxyethyl acrylate and 70-80% ammonium persulfate into the reactor, keep the reaction for 3-5 hours, add the remaining ammonium persulfate, continue to keep the reaction for 1-2 hours, and cool naturally to room temperature to obtain an intermediate; S1.5: Add trimethylhexamethylene diisocyanate to the above intermediate, stir thoroughly, then add the above modified silver powder, continue to stir and mix, and perform ultrasonic treatment at the same time, and obtain a conductive adhesive after vacuum degassing.

[0008] Furthermore, the surface pretreatment of the nano boron nitride powder in step S2 and modification with dopamine hydrochloride specifically comprises the following steps: S2.1: Place sodium hydroxide solution in a heating box, then add nano boron nitride powder into the heating box at a solid-liquid ratio of 1g:25-35mL, heat at a temperature of 100-120°C for 12-16h, and stir with a stirrer to obtain a suspension; S2.2: Filter the suspension, wash the residue with deionized water for 3-5 times, dry it in a vacuum drying oven for 20-24 hours, and grind it to obtain surface pretreated boron nitride powder; S2.3: Add the above-mentioned surface pretreated boron nitride powder and the mixed solution into a mixing box at a solid-liquid ratio of 1g:80-90mL, stir and disperse to obtain a suspension; S2.4: Add dopamine hydrochloride to the above suspension at a solid-liquid ratio of 1g:300-400mL, stir with a stirrer at a rate of 200-300r / min for 4-6h, and obtain modified nano-boron nitride through centrifugal filtration, deionized water washing, drying and grinding.

[0009] Furthermore, the step S4 of adding phenyltriethoxysilane to prepare a modifier and then preparing the insulating coating specifically comprises the following steps: S4.1: Add anhydrous ethanol, anhydrous methanol, hydrochloric acid and deionized water into a reaction box in a volume ratio of 5-6:3-5:1-2:7-8, and stir and mix thoroughly; S4.2: Add phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane to the reaction box, stir and react for 46-48 hours to obtain a precursor solution; S4.3: adding sodium hydroxide solution to the reaction box until the pH of the precursor solution is adjusted to 7-8, then starting the vacuum distillation device in the reaction box to vacuum distill the precursor solution, washing and drying to obtain a modifier; S4.4: dissolve the epoxy resin, the above-mentioned modifier and diaminodiphenylmethane in ether at a mass ratio of 5-8:1-2:1, then add the above-mentioned modified nano boron nitride and modified alumina, mix thoroughly, and obtain an insulating coating.

[0010] Furthermore, step S5 of preparing the substrate and pressing the substrate at room temperature specifically includes the following steps: S5.1: evenly coating the insulating coating obtained in step S4.4 on the upper surface of a copper foil to form an insulating coating, and then laminating another copper foil on the insulating layer. After the insulating coating is dried and cured, a PCB substrate is obtained; S5.2: performing laser drilling processing on a plurality of the above PCB substrates as required, and then electroplating copper filling the drilled holes to obtain pre-processed substrates; S5.3: The conductive adhesive obtained in step S1.5 is evenly coated on the upper surface of the pretreated substrate, and then another pretreated substrate is bonded on the conductive adhesive, and so on, until the required number of layers is reached. After pressing at room temperature, a high-density circuit board with any layer of interconnection is obtained.

[0011] Further, the conductive adhesive includes: 30-40 parts by mass of butyl acrylate, 20-30 parts by mass of methyl methacrylate, 20-30 parts by mass of 2-ethylhexyl acrylate, 8-10 parts by mass of lauryl acrylate, 2-3 parts by mass of γ-methacryloxypropyltrimethoxysilane, 40-50 parts by mass of ethyl acetate, 6-8 parts by mass of β-hydroxyethyl acrylate, 3-5 parts by mass of ammonium persulfate, 1-3 parts by mass of trimethylhexamethylene diisocyanate and 70-80 parts by mass of modified silver powder.

[0012] Furthermore, the mixed solution is prepared by mixing aminomethane buffer and ethanol in a volume ratio of 2-4:1.

[0013] Furthermore, the mass ratio of phenyltriethoxysilane to β-3,4-epoxycyclohexylethyltrimethoxysilane is 6-8:1, and the molar ratio of silane to deionized water is 1:2-3.

[0014] Furthermore, the mass ratios of the modified nano boron nitride and modified alumina to the epoxy resin are 1:20-30 and 1:10-20 respectively.

[0015] A high-density circuit board with arbitrary layer interconnection is prepared by any of the above-mentioned processes for preparing a high-density circuit board with arbitrary layer interconnection.

[0016] Compared with the prior art, the present invention has at least the following beneficial effects: 1. The present invention forms a PCB substrate by compounding two copper foils with an insulating coating, and then uses a conductive adhesive to bond the PCB substrates and press them at room temperature to form a high-density circuit board with arbitrary layers of interconnection. Compared with the traditional circuit board obtained by pressing a prepreg and copper foil layer by layer at high temperature, the present invention has the advantage of being lighter and thinner. At the same time, since the insulating coating has good insulation performance and the conductive adhesive has good conductivity, the obtained high-density circuit board with arbitrary layers of interconnection can work normally under a lighter, thinner and more compact precursor.

[0017] 2. The present invention prepares a conductive adhesive by mixing flaky silver powder and spherical silver powder with γ-glycidyloxypropyltrimethoxysilane in a certain proportion for modification, and then fully mixing the mixture with an intermediate prepared from butyl acrylate, methyl methacrylate, 2-ethylhexyl acrylate and lauryl acrylate as raw materials. The volume resistivity of the conductive adhesive can be effectively reduced to improve its conductivity. In addition, the conductive adhesive has excellent holding force, thereby extending the service life of the circuit board.

[0018] 3. The present invention prepares a modifier by using phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane as raw materials, and then mixes it with epoxy resin. The epoxy resin is modified to improve the adhesion of the epoxy resin. Then, by adding modified alumina, the adhesion and insulation performance of the prepared insulating coating can be further improved, and the copper foil can be prevented from falling off, so as to extend the service life of the circuit board.

[0019] 4. The present invention first mixes nano boron nitride powder with sodium hydroxide solution for surface pretreatment, then mixes with dopamine hydrochloride for modification, and then adds the modified nano boron nitride to epoxy resin, which can improve the insulation performance of the obtained insulating coating, thereby ensuring the normal operation of the obtained high-density circuit board with any layer of interconnection. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.

[0021] Figure 1 The present invention is a flowchart of the process for preparing a high-density circuit board with arbitrary layer interconnections adopted in an embodiment of the present invention.

[0022] Figure 2 This is a summary table of performance test results of Examples 1-3 of the present invention.

[0023] Figure 3 The following is a summary table of the comparison results between Example 1 of the present invention and Comparative Example 1.

[0024] Figure 4 The following is a summary table of the comparison results between Example 1 and Comparative Example 2 of the present invention.

[0025] Figure 5 The following is a summary table of the comparison results between Example 1 of the present invention and Comparative Examples 3 and 4.

[0026] Figure 6 The following is a summary table of the comparison results between Example 1 of the present invention and Comparative Example 5. DETAILED DESCRIPTION

[0027] The following is a detailed description of an arbitrary layer interconnection high-density circuit board and its preparation process provided by the present invention in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and the accompanying drawings are only for a more specific description of the embodiments, and are not intended to specifically limit the present invention. Example 1

[0028] A process for preparing a high-density circuit board with arbitrary layer interconnection, such as Figure 1 As shown, the following steps are included: S1: Modification of silver powder and preparation of conductive adhesive The flaky silver powder and the spherical silver powder were added to a planetary centrifugal mixer at a mass ratio of 3:6, and then anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane accounting for 3% of the total mass of the flaky silver powder and the spherical silver powder were added at a solid-liquid ratio of 1g:10mL, and the mixture was stirred and mixed evenly, and then placed in an oven and dried at 60°C for 2h to obtain modified silver powder for standby use, and then 30 parts by mass of butyl acrylate, 20 parts by mass of methyl methacrylate, 20 parts by mass of 2-ethylhexyl acrylate and 8 parts by mass of lauryl acrylate were added to a mixing tank, and then 2 parts by mass of γ-methacryloxypropyltrimethoxysilane and 40 parts by mass of ethyl acetate were added to the mixing tank, and the mixture was fully stirred and mixed to obtain a premixed solution, and then, the premixed solution was added to the reaction mixture. Nitrogen is introduced into the reactor until the air is exhausted, and then 2 / 3 of the premixed liquid is added to the reactor, heated at 70°C for 30min, and stirred at a rate of 300r / min, then the stirring rate is adjusted to 100r / min, and the remaining premixed liquid, 6 parts by mass of β-hydroxyethyl acrylate and 2 parts by mass of ammonium persulfate are added to the reactor, and after the reaction is kept warm for 3h, the remaining ammonium persulfate is added, and the reaction is continued for 1h, and it is naturally cooled to room temperature to obtain an intermediate, and then 1 part by mass of trimethylhexamethylene diisocyanate is added to the intermediate, and it is fully stirred, and then 70 parts by mass of modified silver powder are added, and stirring and mixing are continued, and ultrasonic treatment is performed at the same time. After vacuum degassing, a conductive adhesive is obtained; S2: Surface pretreatment of nano-boron nitride powder and modification with dopamine hydrochloride Put the sodium hydroxide solution into a heating box, then add the nano boron nitride powder into the heating box at a solid-liquid ratio of 1g:25mL, heat at a temperature of 100°C for 12h, and stir with a stirrer to obtain a suspension, then filter the suspension, wash the filter residue with deionized water for 3 times, and dry it in a vacuum drying box for 20h. After grinding, obtain surface pretreated boron nitride powder, then add the surface pretreated boron nitride powder and a mixed solution prepared by mixing aminomethane buffer and ethanol in a volume ratio of 2:1 into a mixing box at a solid-liquid ratio of 1g:80mL, stir and disperse to obtain a suspension, then add dopamine hydrochloride into the suspension at a solid-liquid ratio of 1g:300mL, stir with a stirrer at a rate of 200r / min for 4h, centrifuge, wash with deionized water, dry and grind to obtain modified nano boron nitride; S3: γ-glycidyloxypropyltrimethoxysilane activated alumina Dissolve γ-glycidyloxypropyltrimethoxysilane in ethanol, add acetic acid until the pH is adjusted to 3, then add alumina, heat reflux at 60°C and stir for 5 hours, cool naturally to room temperature, filter, wash with ethanol and dry to obtain activated alumina; S4: Add phenyltriethoxysilane to prepare a modifier and then prepare an insulating coating Anhydrous ethanol, anhydrous methanol, hydrochloric acid and deionized water are added to a reaction box in a volume ratio of 5:3:1:7, and the mixture is fully stirred. Phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane in a mass ratio of 6:1 are then added to the reaction box, wherein the molar ratio of silane to deionized water is 1:2, and the reaction is stirred for 46 hours to obtain a precursor solution. Sodium hydroxide solution is then added to the reaction box until the pH of the precursor solution is adjusted to 7, and then a vacuum distillation device in the reaction box is started to vacuum distill the precursor solution, and a modifier is obtained after washing and drying. Subsequently, epoxy resin, modifier and diaminodiphenylmethane are dissolved in ether in a mass ratio of 5:1:1, and the above-mentioned modified nano boron nitride and modified alumina are added, wherein the mass ratios of modified nano boron nitride and modified alumina to epoxy resin are 1:20 and 1:10, respectively. After fully mixing, an insulating coating is obtained. S5: Prepare substrate and press the substrate at room temperature The insulating coating is evenly coated on the upper surface of a copper foil to form an insulating coating, and then another copper foil is attached to the insulating layer. After the insulating coating is dried and cured, a PCB substrate with an insulating coating thickness of about 40 μm is obtained. Then, laser drilling is performed on several PCB substrates as required, and the drilled holes are electroplated with copper to obtain a pre-treated substrate. The conductive adhesive is evenly coated on the upper surface of the pre-treated substrate, and then another pre-treated substrate is attached to the conductive adhesive, and so on, until the required number of layers is reached. After pressing at room temperature, a high-density circuit board with any layer of interconnection is obtained.

[0029] Insulation coating performance test: First, the insulating coating is evenly coated on the surface of the copper foil. After it is cured, a 15cm×10cm copper foil with insulating coating on the surface is taken, the test voltage is set to 250V, and the volume resistivity is measured using a high resistance meter. The results are as follows: Figure 2 shown.

[0030] Then, the adhesion test was carried out according to GB / T9286-2021, and the results were as follows: Figure 2 As shown; Conductive adhesive performance test: First, the conductive adhesive is coated on the upper surface of the copper foil. After curing, its adhesion is tested according to GB / T4851-1998 standard. The results are as follows: Figure 2 As shown; Then, the conductive adhesive was coated in a mold of 20 mm×20 mm×0.5 mm, and after curing, its volume resistivity was tested using a four-probe tester. Example 2

[0031] A process for preparing a high-density circuit board with arbitrary layer interconnection, such as Figure 1 As shown, the following steps are included: S1: Modification of silver powder and preparation of conductive adhesive The flaky silver powder and the spherical silver powder were added to a planetary centrifugal mixer at a mass ratio of 4:7, and then anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane accounting for 4% of the total mass of the flaky silver powder and the spherical silver powder were added at a solid-liquid ratio of 1g:11mL, and the mixture was stirred and mixed evenly, and then placed in an oven and dried at 70°C for 2.5h to obtain modified silver powder for standby use, and then 35 parts by mass of butyl acrylate, 25 parts by mass of methyl methacrylate, 25 parts by mass of 2-ethylhexyl acrylate and 9 parts by mass of lauryl acrylate were added to a mixing tank, and then 2 parts by mass of γ-methacryloxypropyltrimethoxysilane and 45 parts by mass of ethyl acetate were added to the mixing tank, and the mixture was fully stirred and mixed to obtain a premixed solution, and then, the premixed solution was added to the reverse flaky silver powder. Nitrogen is introduced into the reactor until the air is exhausted, and then 2 / 3 of the premixed liquid is added to the reactor, heated at 75°C for 35 minutes, and stirred at a rate of 350 r / min, and then the stirring rate is adjusted to 150 r / min, and the remaining premixed liquid, 7 parts by mass of β-hydroxyethyl acrylate and 3 parts by mass of ammonium persulfate are added to the reactor, and after the reaction is kept warm for 4 hours, the remaining ammonium persulfate is added, and the reaction is continued for 1.5 hours. It is naturally cooled to room temperature to obtain an intermediate, and then 2 parts by mass of trimethylhexamethylene diisocyanate are added to the intermediate, and it is fully stirred, and then 75 parts by mass of modified silver powder are added, and stirring and mixing are continued. Ultrasonic treatment is performed at the same time, and after vacuum degassing, a conductive adhesive is obtained; S2: Surface pretreatment of nano-boron nitride powder and modification with dopamine hydrochloride Put the sodium hydroxide solution into a heating box, then add the nano boron nitride powder into the heating box at a solid-liquid ratio of 1g:30mL, heat at a temperature of 110°C for 14h, and stir with a stirrer to obtain a suspension, then filter the suspension, wash the filter residue with deionized water for 4 times, and place it in a vacuum drying box for 22h. After grinding, the surface pretreated boron nitride powder is obtained, and then the surface pretreated boron nitride powder and a mixed solution prepared by mixing aminomethane buffer and ethanol in a volume ratio of 3:1 are added to a mixing box at a solid-liquid ratio of 1g:85mL, stirred and dispersed to obtain a suspension, and then dopamine hydrochloride is added to the suspension at a solid-liquid ratio of 1g:350mL, and stirred with a stirrer at a rate of 250r / min for 5h, and modified nano boron nitride is obtained after centrifugal filtration, deionized water washing, drying and grinding; S3: γ-glycidyloxypropyltrimethoxysilane activated alumina Dissolve γ-glycidyloxypropyltrimethoxysilane in ethanol, add acetic acid until the pH is adjusted to 3.5, then add alumina, heat reflux at 65° C. and stir for 5.5 hours, cool naturally to room temperature, filter, wash with ethanol and dry to obtain activated alumina; S4: Add phenyltriethoxysilane to prepare a modifier and then prepare an insulating coating Anhydrous ethanol, anhydrous methanol, hydrochloric acid and deionized water are added to a reaction box in a volume ratio of 5:4:1:8, and the mixture is fully stirred. Phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane in a mass ratio of 7:1 are then added to the reaction box, wherein the molar ratio of silane to deionized water is 1:2, and the mixture is stirred for reaction for 47 hours to obtain a precursor solution. Sodium hydroxide solution is then added to the reaction box until the pH of the precursor solution is adjusted to 7.5. A vacuum distillation device in the reaction box is then started to vacuum distill the precursor solution, and a modifier is obtained after washing and drying. Subsequently, epoxy resin, modifier and diaminodiphenylmethane are dissolved in ether in a mass ratio of 6:1:1, and the modified nano boron nitride and modified alumina are added, wherein the mass ratios of the modified nano boron nitride and modified alumina to the epoxy resin are 1:25 and 1:15, respectively. After fully mixing, an insulating coating is obtained. S5: Prepare substrate and press the substrate at room temperature The insulating coating is evenly coated on the upper surface of a copper foil to form an insulating coating, and then another copper foil is attached to the insulating layer. After the insulating coating is dried and cured, a PCB substrate with an insulating coating thickness of about 45 μm is obtained. Then, laser drilling is performed on several PCB substrates as required, and the drilled holes are electroplated with copper to obtain a pre-treated substrate. The conductive adhesive is evenly coated on the upper surface of the pre-treated substrate, and then another pre-treated substrate is attached to the conductive adhesive, and so on, until the required number of layers is reached. After pressing at room temperature, a high-density circuit board with any layer of interconnection is obtained.

[0032] Insulation coating performance test: First, the insulating coating is evenly coated on the surface of the copper foil. After it is cured, a 15cm×10cm copper foil with insulating coating on the surface is taken, the test voltage is set to 250V, and the volume resistivity is measured using a high resistance meter. The results are as follows: Figure 2 shown.

[0033] Then, the adhesion test was carried out according to GB / T9286-2021, and the results were as follows: Figure 2 As shown; Conductive adhesive performance test: First, the conductive adhesive is coated on the upper surface of the copper foil. After curing, its adhesion is tested according to GB / T4851-1998 standard. The results are as follows: Figure 2 As shown; Then, the conductive adhesive was coated in a 20 mm × 20 mm × 0.5 mm mold. After curing, the volume resistivity was tested using a four-probe tester. The results are as follows: Figure 2 shown. Example 3

[0034] A process for preparing a high-density circuit board with arbitrary layer interconnection, such as Figure 1 As shown, the following steps are included: S1: Modification of silver powder and preparation of conductive adhesive The flaky silver powder and the spherical silver powder were added to a planetary centrifugal mixer at a mass ratio of 5:8, and then anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane accounting for 5% of the total mass of the flaky silver powder and the spherical silver powder were added at a solid-liquid ratio of 1g:12mL, and the mixture was stirred and mixed evenly, and then placed in an oven and dried at 80°C for 3h to obtain modified silver powder for standby use, and then 40 parts by mass of butyl acrylate, 30 parts by mass of methyl methacrylate, 30 parts by mass of 2-ethylhexyl acrylate and 10 parts by mass of lauryl acrylate were added to a mixing tank, and then 3 parts by mass of γ-methacryloxypropyltrimethoxysilane and 50 parts by mass of ethyl acetate were added to the mixing tank, and the mixture was fully stirred and mixed to obtain a premixed solution, and then, Nitrogen was introduced into the reactor until the air was exhausted, and then 2 / 3 of the premixed liquid was added to the reactor, heated at 80° C. for 40 min, and stirred at a rate of 400 r / min, and then the stirring rate was adjusted to 200 r / min, and the remaining premixed liquid, 8 parts by mass of β-hydroxyethyl acrylate and 4 parts by mass of ammonium persulfate were added to the reactor, and after the reaction was kept warm for 5 hours, the remaining ammonium persulfate was added, and the reaction was continued for 2 hours, and naturally cooled to room temperature to obtain an intermediate, and then 3 parts by mass of trimethylhexamethylene diisocyanate was added to the intermediate, and the mixture was fully stirred, and then 80 parts by mass of modified silver powder were added, and the stirring and mixing were continued, and ultrasonic treatment was performed at the same time, and a conductive adhesive was obtained after vacuum degassing; S2: Surface pretreatment of nano-boron nitride powder and modification with dopamine hydrochloride Put the sodium hydroxide solution into a heating box, then add the nano boron nitride powder into the heating box at a solid-liquid ratio of 1g:35mL, heat at a temperature of 120°C for 16h, and stir with a stirrer to obtain a suspension, then filter the suspension, wash the filter residue with deionized water for 5 times, and place it in a vacuum drying box for 24h. After grinding, obtain surface pretreated boron nitride powder, then add the surface pretreated boron nitride powder and a mixed solution prepared by mixing aminomethane buffer and ethanol in a volume ratio of 4:1 into a mixing box at a solid-liquid ratio of 1g:90mL, stir and disperse to obtain a suspension, then add dopamine hydrochloride into the suspension at a solid-liquid ratio of 1g:400mL, stir with a stirrer at a rate of 300r / min for 6h, centrifuge, wash with deionized water, dry and grind to obtain modified nano boron nitride; S3: γ-glycidyloxypropyltrimethoxysilane activated alumina Dissolve γ-glycidyloxypropyltrimethoxysilane in ethanol, add acetic acid until the pH is adjusted to 4, then add alumina, heat reflux at 70°C and stir for 6 hours, cool naturally to room temperature, filter, wash with ethanol and dry to obtain activated alumina; S4: Add phenyltriethoxysilane to prepare a modifier and then prepare an insulating coating Anhydrous ethanol, anhydrous methanol, hydrochloric acid and deionized water are added to a reaction box in a volume ratio of 6:5:2:8, and the mixture is fully stirred. Phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane in a mass ratio of 8:1 are then added to the reaction box, wherein the molar ratio of silane to deionized water is 1:3, and the mixture is stirred for 48 hours to obtain a precursor solution. Sodium hydroxide solution is then added to the reaction box until the pH of the precursor solution is adjusted to 8, and then a vacuum distillation device in the reaction box is started to vacuum distill the precursor solution, and the modifier is obtained after washing and drying. Subsequently, epoxy resin, modifier and diaminodiphenylmethane are dissolved in ether in a mass ratio of 8:2:1, and the modified nano boron nitride and modified alumina are added, wherein the mass ratios of the modified nano boron nitride and the modified alumina to the epoxy resin are 1:30 and 1:20, respectively. After fully mixing, an insulating coating is obtained. S5: Prepare substrate and press the substrate at room temperature The insulating coating is evenly coated on the upper surface of a copper foil to form an insulating coating, and then another copper foil is attached to the insulating layer. After the insulating coating is dried and cured, a PCB substrate with an insulating coating thickness of about 50 μm is obtained. Then, laser drilling is performed on several PCB substrates as required, and the drilled holes are electroplated with copper to obtain a pre-treated substrate. The conductive adhesive is evenly coated on the upper surface of the pre-treated substrate, and then another pre-treated substrate is attached to the conductive adhesive, and so on, until the required number of layers is reached. After pressing at room temperature, a high-density circuit board with any layer of interconnection is obtained.

[0035] Insulation coating performance test: First, the insulating coating is evenly coated on the surface of the copper foil. After it is cured, a 15cm×10cm copper foil with insulating coating on the surface is taken, the test voltage is set to 250V, and the volume resistivity is measured using a high resistance meter. The results are as follows: Figure 2 shown.

[0036] Then, the adhesion test was carried out according to GB / T9286-2021, and the results were as follows: Figure 2 As shown; Conductive adhesive performance test: First, the conductive adhesive is coated on the upper surface of the copper foil. After curing, its adhesion is tested according to GB / T4851-1998 standard. The results are as follows: Figure 2As shown; Then, the conductive adhesive was coated in a 20 mm × 20 mm × 0.5 mm mold. After curing, the volume resistivity was tested using a four-probe tester. The results are as follows: Figure 2 shown. Comparative Example 1

[0037] The thickness of the commercially available prepreg was compared with the thickness of the insulating coating of Example 1. The results are as follows: Figure 3 shown.

[0038] from Figure 2 and Figure 3 It can be seen that by compounding two copper foils with insulating coating to form a PCB substrate, and then bonding the PCB substrates with a conductive adhesive and pressing them at room temperature at one time to form an arbitrary layer interconnected high-density circuit board, compared with the traditional circuit board obtained by pressing the semi-cured sheet and copper foil layer by layer at high temperature, it has the advantage of being lighter and thinner. At the same time, since the insulating coating has good insulating properties and the conductive adhesive has good conductivity, the obtained arbitrary layer interconnected high-density circuit board can work normally under a lighter, thinner and smaller precursor. Comparative Example 2

[0039] The difference between this comparative example and Example 1 is that only the flaky silver powder in step S1 is replaced with an equal amount of spherical silver powder, and then the conductive properties of the conductive adhesive are tested according to the performance test method in Example 1. The results are as follows: Figure 4 shown.

[0040] from Figure 2 and Figure 4 It can be seen that the conductive adhesive is prepared by mixing flaky silver powder and spherical silver powder with γ-glycidyloxypropyltrimethoxysilane in a certain proportion for modification, and then fully mixing with an intermediate prepared with butyl acrylate, methyl methacrylate, 2-ethylhexyl acrylate and lauryl acrylate as raw materials. The volume resistivity of the conductive adhesive can be effectively reduced, thereby achieving the effect of improving its conductivity. In addition, the conductive adhesive also has excellent adhesion, thereby extending the service life of the circuit board. Comparative Example 3

[0041] The difference between this comparative example and Example 1 is that the step of preparing the modifier in step S4 is removed, that is, epoxy resin and diaminodiphenylmethane are directly dissolved in ether, and then modified nano boron nitride and modified alumina are added to prepare an insulating coating. Then, the insulating coating prepared in this comparative example 3 is tested for performance according to the insulating coating performance test method in Example 1. The results are shown in FIG. Figure 5 shown.

[0042] From the comparison of performance test results, it can be seen that the adhesion of epoxy resin can be improved by preparing the modifier with phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane as raw materials and then mixing it with epoxy resin to modify the epoxy resin. Comparative Example 4

[0043] The difference between this comparative example and Example 1 is that the modified alumina in step S4 is removed, and then the adhesion of the insulating coating prepared in this comparative example 4 is tested according to the insulating coating adhesion test method in Example 1. The results are as follows: Figure 5 shown.

[0044] From the comparison of the test results, it can be seen that by adding modified alumina, the adhesion and insulation performance of the prepared insulating coating can be further improved, the copper foil can be prevented from falling off, and the service life of the circuit board can be extended. Comparative Example 5

[0045] The difference between this comparative example and Example 1 is that step S2 is removed, and the modified nano boron nitride in step S4 is removed. Then, the insulating performance of the insulating coating prepared in this comparative example 5 is tested according to the insulating performance test method of the insulating coating in Example 1. The results are as follows: Figure 6 shown.

[0046] It can be seen from the performance test results that by first mixing the nano-boron nitride powder with sodium hydroxide solution for surface pretreatment, then mixing with dopamine hydrochloride for modification, and adding the modified nano-boron nitride to epoxy resin, the insulation performance of the insulating coating can be improved, thereby ensuring the normal operation of the prepared high-density circuit board with any layer of interconnection.

[0047] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A process for preparing a high-density circuit board with arbitrary layer interconnection, characterized in that: The steps include: S1: Modification of silver powder and preparation of conductive adhesive Adding γ-glycidyloxypropyltrimethoxysilane to flaky silver powder and spherical silver powder to prepare modified silver powder, then using butyl acrylate, methyl methacrylate, 2-ethylhexyl acrylate and lauryl acrylate as raw materials to prepare an intermediate, and then adding the modified silver powder to the intermediate to obtain a conductive adhesive; S2: Surface pretreatment of nano-boron nitride powder and modification with dopamine hydrochloride The nano boron nitride powder and the sodium hydroxide solution are heated and stirred to pre-treat the surface of the nano boron nitride powder, and then the nano boron nitride powder is uniformly mixed with the mixed solution, and dopamine hydrochloride is added for modification to obtain modified nano boron nitride; S3: γ-glycidyloxypropyltrimethoxysilane activated alumina Dissolve γ-glycidyloxypropyltrimethoxysilane in ethanol, add acetic acid until the pH is adjusted to 3-4, then add alumina, heat reflux at 60-70° C. and stir for 5-6 hours, cool naturally to room temperature, filter, wash with ethanol and dry to obtain activated alumina; S4: Add phenyltriethoxysilane to prepare a modifier and then prepare an insulating coating Anhydrous ethanol, anhydrous methanol, hydrochloric acid, deionized water, phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane are mixed to prepare a modifier, which is then mixed with epoxy resin, diaminodiphenylmethane, the modified nano boron nitride and the modified alumina to obtain an insulating coating; S5: Prepare substrate and press the substrate at room temperature The above-mentioned insulating coating is coated on the upper surface of the copper foil, and then another copper foil is attached to form a PCB substrate. After the PCB substrate is laser drilled and filled with copper by electroplating, it is bonded with the above-mentioned conductive adhesive and pressed at room temperature to obtain a high-density circuit board with arbitrary layer interconnections.

2. The process for preparing a high-density circuit board with arbitrary layer interconnection according to claim 1, characterized in that: The modified silver powder and the preparation of the conductive adhesive in step S1 specifically include the following steps: S1.1: Add flaky silver powder and spherical silver powder into a planetary centrifugal mixer at a mass ratio of 3-5:6-8, then add anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane accounting for 3-5% of the total mass of flaky silver powder and spherical silver powder at a solid-liquid ratio of 1g:10-12mL, stir and mix evenly, then place in an oven and dry at 60-80°C for 2-3h to obtain modified silver powder; S1.2: Add butyl acrylate, methyl methacrylate, 2-ethylhexyl acrylate and lauryl acrylate into a mixing tank, then add γ-methacryloxypropyltrimethoxysilane and ethyl acetate into the mixing tank, stir and mix thoroughly to obtain a premixed solution; S1.3: nitrogen is introduced into the reactor until all the air is exhausted, and then 2 / 3 of the premixed liquid is added into the reactor, and heated at 70-80°C for 30-40 min, while stirring at a rate of 300-400 r / min; S1.4: Adjust the stirring rate to 100-200 r / min, add the remaining premix, β-hydroxyethyl acrylate and 70-80% ammonium persulfate into the reactor, keep the reaction for 3-5 hours, add the remaining ammonium persulfate, continue to keep the reaction for 1-2 hours, and cool naturally to room temperature to obtain an intermediate; S1.5: Add trimethylhexamethylene diisocyanate to the above intermediate, stir thoroughly, then add the above modified silver powder, continue to stir and mix, and perform ultrasonic treatment at the same time, and obtain a conductive adhesive after vacuum degassing.

3. The process for preparing a high-density circuit board with arbitrary layer interconnection according to claim 2, characterized in that: Step S2 is to pre-treat the surface of the nano boron nitride powder and modify it with dopamine hydrochloride, which specifically includes the following steps: S2.1: Place sodium hydroxide solution in a heating box, then add nano boron nitride powder into the heating box at a solid-liquid ratio of 1g:25-35mL, heat at a temperature of 100-120°C for 12-16h, and stir with a stirrer to obtain a suspension; S2.2: Filter the suspension, wash the residue with deionized water for 3-5 times, dry it in a vacuum drying oven for 20-24 hours, and grind it to obtain surface pretreated boron nitride powder; S2.3: Add the above-mentioned surface pretreated boron nitride powder and the mixed solution into a mixing box at a solid-liquid ratio of 1g:80-90mL, stir and disperse to obtain a suspension; S2.4: Add dopamine hydrochloride to the above suspension at a solid-liquid ratio of 1g:300-400mL, stir with a stirrer at a rate of 200-300r / min for 4-6h, and obtain modified nano-boron nitride through centrifugal filtration, deionized water washing, drying and grinding.

4. The process for preparing a high-density circuit board with arbitrary layer interconnection according to claim 3, characterized in that: Step S4 of adding phenyltriethoxysilane to prepare a modifier and then preparing the insulating coating specifically comprises the following steps: S4.1: Add anhydrous ethanol, anhydrous methanol, hydrochloric acid and deionized water into a reaction box in a volume ratio of 5-6:3-5:1-2:7-8, and stir and mix thoroughly; S4.2: Add phenyltriethoxysilane and β-3,4-epoxycyclohexylethyltrimethoxysilane to the reaction box, stir and react for 46-48 hours to obtain a precursor solution; S4.3: adding sodium hydroxide solution to the reaction box until the pH of the precursor solution is adjusted to 7-8, then starting the vacuum distillation device in the reaction box to vacuum distill the precursor solution, washing and drying to obtain a modifier; S4.4: dissolve the epoxy resin, the above-mentioned modifier and diaminodiphenylmethane in ether at a mass ratio of 5-8:1-2:1, then add the above-mentioned modified nano boron nitride and modified alumina, mix thoroughly, and obtain an insulating coating.

5. The process for preparing a high-density circuit board with arbitrary layer interconnection according to claim 4, characterized in that: Step S5 of preparing the substrate and pressing the substrate at room temperature specifically includes the following steps: S5.1: evenly coating the insulating coating obtained in step S4.4 on the upper surface of a copper foil to form an insulating coating, and then laminating another copper foil on the insulating layer. After the insulating coating is dried and cured, a PCB substrate is obtained; S5.2: performing laser drilling processing on a plurality of the above PCB substrates as required, and then electroplating copper filling the drilled holes to obtain pre-processed substrates; S5.3: The conductive adhesive obtained in step S1.5 is evenly coated on the upper surface of the pretreated substrate, and then another pretreated substrate is bonded on the conductive adhesive, and so on, until the required number of layers is reached. After pressing at room temperature, a high-density circuit board with any layer of interconnection is obtained.

6. The process for preparing a high-density circuit board with arbitrary layer interconnection according to claim 2, characterized in that: The conductive adhesive includes: 30-40 parts by mass of butyl acrylate, 20-30 parts by mass of methyl methacrylate, 20-30 parts by mass of 2-ethylhexyl acrylate, 8-10 parts by mass of lauryl acrylate, 2-3 parts by mass of γ-methacryloxypropyltrimethoxysilane, 40-50 parts by mass of ethyl acetate, 6-8 parts by mass of β-hydroxyethyl acrylate, 3-5 parts by mass of ammonium persulfate, 1-3 parts by mass of trimethylhexamethylene diisocyanate and 70-80 parts by mass of modified silver powder.

7. The process for preparing a high-density circuit board with arbitrary layer interconnection according to claim 3, characterized in that: The mixed solution is prepared by mixing aminomethane buffer and ethanol in a volume ratio of 2-4:

1.

8. The process for preparing a high-density circuit board with arbitrary layer interconnection according to claim 4, characterized in that: The mass ratio of phenyltriethoxysilane to β-3,4-epoxycyclohexylethyltrimethoxysilane is 6-8:1, and the molar ratio of silane to deionized water is 1:2-3.

9. The process for preparing a high-density circuit board with arbitrary layer interconnection according to claim 4, characterized in that: The mass ratios of the modified nano boron nitride and the modified alumina to the epoxy resin are 1:20-30 and 1:10-20 respectively.

10. A high-density circuit board with arbitrary layer interconnection, characterized in that: It is prepared by the preparation process of a high-density circuit board with arbitrary layer interconnection as described in any one of claims 1-9.

Citation Information

Patent Citations

  • Acrylic ester modified epoxy resin conductive chip adhesive

    CN103242775A

  • Arbitrary layer interconnection circuit board and preparation method thereof

    CN117279187A

  • Electrically conductive adhesive and wiring board using the same

    JP2001115127A

  • Conductive adhesive composition

    JP2005132854A