Anti-reflection film, preparation method thereof and perovskite photovoltaic module
A room temperature anti-reflection film preparation method for perovskite photovoltaic modules addresses glass warping and deformation issues, enhancing light transmittance and power generation efficiency while reducing energy consumption and equipment costs.
Patent Information
- Application Number
- CN202310634478.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
Existing anti-reflection films for perovskite photovoltaic modules require high-temperature coating processes that cause glass warping and deformation, affecting the subsequent perovskite cell process preparation and performance.
A method for preparing an anti-reflection film at room temperature on encapsulated perovskite photovoltaic modules using an anti-reflection coating liquid composed of organosilicon monomer, alkali catalyst, template agent, and solvent, followed by room temperature curing, washing, and drying, which avoids high-temperature sintering issues.
The method prevents glass warping, enhances light transmittance, improves mechanical properties, and increases power generation efficiency of perovskite photovoltaic modules while reducing energy consumption and equipment costs.
Smart Images

Figure CN119072198A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of perovskite photovoltaic modules, and in particular to an anti-reflection film and a preparation method thereof, and a perovskite photovoltaic module. Background Art
[0002] With the development of photovoltaic technology, AR anti-reflection coatings technology has also received attention. With the current FTO float glass production process, the best glass with a transmittance of only 80% to 84%, and about 15% to 20% of sunlight is not transmitted or is reflected (such as Figure 1 As shown in the figure, it cannot be transferred to the perovskite chip to generate electricity. In order to improve the utilization rate of sunlight, crystalline silicon solar cell modules generally add one or more layers of anti-reflection film on the surface of the front panel tempered or heat-strengthened glass to reduce the reflection of light. The preparation of existing anti-reflection films mainly uses high-temperature coating liquid, so they can only be applied before the component is packaged (because coating after packaging will cause the packaging film to age and damage), and high temperature will inevitably cause the glass to deform, that is, the glass will warp, the waveform will be large, and other problems will occur, affecting the subsequent perovskite cell process preparation and the performance of the perovskite cell.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] One object of the present invention is to provide a method for preparing an anti-reflection film to solve the technical problems in the prior art of using a high-temperature coating solution to prepare an anti-reflection film before product packaging, such as glass warping and large waveform curvature, which affect the subsequent perovskite battery process preparation.
[0005] Another object of the present invention is to provide an anti-reflection film having a uniform, dense and flat film layer, strong mechanical properties, high porosity and large light transmittance gain.
[0006] Another object of the present invention is to provide a perovskite photovoltaic module.
[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0008] The method for preparing an anti-reflection film comprises the following steps:
[0009] The anti-reflection coating liquid is coated on the glass surface of the encapsulated perovskite photovoltaic module substrate; and then the room temperature curing, washing treatment and drying treatment are carried out in sequence.
[0010] In one embodiment, before applying the anti-reflection coating liquid, the method further includes: preheating the packaged perovskite photovoltaic module substrate.
[0011] In one embodiment, the preheating treatment specifically includes: heating the packaged perovskite photovoltaic module substrate to 40-80° C. and keeping the temperature for 10-30 minutes.
[0012] In one embodiment, after the preheating treatment, the method further includes: continuously performing heat treatment on the encapsulated perovskite photovoltaic module substrate.
[0013] In one embodiment, the continuous heat treatment maintains the temperature of the encapsulated perovskite photovoltaic module substrate at 40-80°C.
[0014] In one embodiment, the anti-reflective coating liquid includes an organosilicon monomer, an alkali catalyst, a template agent and a solvent; wherein the molar number of the organosilicon monomer accounts for 1% to 5% of the total molar number of the anti-reflective coating liquid, the molar number of the alkali catalyst accounts for 1% to 3% of the total molar number of the anti-reflective coating liquid, the molar number of the template agent accounts for 0.1% to 0.5% of the total molar number of the anti-reflective coating liquid, and the molar number of the solvent accounts for 98% to 91.5% of the total molar number of the anti-reflective coating liquid.
[0015] In one embodiment, the silicone monomer includes at least one of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, octyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, chloropropyltriethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0016] In one embodiment, the base catalyst includes at least one of ammonia water, tetramethylammonium hydroxide, sodium hydroxide, potassium hydroxide, acrylamide, ethylenediamine, hexamethylenediamine and triethylamine.
[0017] In one embodiment, the templating agent comprises an alkylammonium bromide.
[0018] In one embodiment, the solvent includes at least one of ethanol, water, isopropanol, tert-butyl alcohol, ethylene glycol and glycerol.
[0019] In one embodiment, the method for preparing the anti-reflective coating solution includes: mixing an alkali catalyst, a template agent and a solvent to obtain a first mixed solution; adding an organosilicon monomer dropwise to the first mixed solution, and then performing stirring and aging treatments.
[0020] In one embodiment, the stirring treatment time is 2 to 4 hours.
[0021] In one embodiment, the aging treatment time is 20 to 25 hours.
[0022] In one embodiment, the coating method includes at least one of roller coating, spray coating and Czochralski method.
[0023] In one embodiment, the room temperature curing temperature is 18 to 30° C., and the room temperature curing time is 5 to 30 minutes.
[0024] In one embodiment, the washing treatment uses ethanol and / or water.
[0025] An anti-reflection film is prepared by the anti-reflection film preparation method; the thickness of the anti-reflection film is 80-120nm.
[0026] A perovskite photovoltaic module comprises a perovskite photovoltaic module substrate and an anti-reflection film arranged on the float glass surface of the perovskite photovoltaic module substrate; the anti-reflection film is the anti-reflection film as described above or the anti-reflection film prepared by the preparation method of the anti-reflection film.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The method of the present invention can avoid the problems of large warping and large waveform curvature of FTO glass caused by high-temperature sintering; can solve the problem of low transmittance of FTO glass, improve visible light transmittance, and increase the output power (photoelectric conversion efficiency) of perovskite thin film batteries; can avoid the contamination of the FTO conductive layer caused by water or alcohol cleaning after the anti-reflection film coating process is used alone, the increase in square resistance and the internal defects of the battery caused by pollutants; can solve the problem that high-temperature sintering anti-reflection film cannot be used after perovskite thin film battery packaging; the method of preparing anti-reflection film at room temperature can reduce energy consumption and save equipment development funds.
[0029] (2) The anti-reflection film of the present invention has a uniform, dense and flat film layer, strong mechanical properties, high porosity, and large light transmittance gain.
[0030] (3) The perovskite photovoltaic module of the present invention has high light transmittance gain and high power gain. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 IU curve and power curve of the perovskite photovoltaic module and the perovskite photovoltaic module base member of Example 1 of the present invention;
[0033] Figure 2 It is a schematic diagram of the structure of the perovskite photovoltaic module of the present invention. DETAILED DESCRIPTION
[0034] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0035] According to one aspect of the present invention, the present invention relates to a method for preparing an anti-reflection film for a perovskite photovoltaic module, comprising the following steps:
[0036] The anti-reflection coating liquid is coated on the glass surface of the encapsulated perovskite photovoltaic module substrate; and then the room temperature curing, washing treatment and drying treatment are carried out in sequence.
[0037] After the perovskite photovoltaic module base is packaged, the present invention coats the light-receiving surface (float glass) of the FTO film layer with an anti-reflection coating liquid under low temperature conditions, which can reduce the difficulty of production and preparation, reduce the investment in tempering equipment, and solve the high energy consumption problem caused by high-temperature curing and tempering. The anti-reflection film prepared by low-temperature coating can improve the transmittance of FTO glass, increase the power gain generated by the photovoltaic effect of perovskite, effectively increase the power generation, and increase economic benefits. The present invention adopts room temperature curing treatment to reduce the influence of high-temperature curing process on the thermal stability of perovskite cells to improve battery performance. The present invention washes after curing treatment to achieve a porous structure of the coating layer. If it is not washed, the template agent still remains, and the pores formed by the accumulation of silica formed by base catalysis are used to reduce the refractive index, and the gain effect is low. The present invention does not need to pre-synthesize hollow silica microspheres, and uses a "one-pot method" to directly generate a coating layer with holes on the glass surface. It is simple to operate, strong in practicality, low in cost, and suitable for large-scale production.
[0038] The perovskite photovoltaic module substrate of the present invention has been packaged by lamination process, lamination + autoclave process, vacuum bag + autoclave process, and roller pressing + autoclave process. The perovskite photovoltaic module substrate includes a perovskite cell, a first surface of the perovskite cell is sequentially stacked with an FTO film layer and a float glass, and a second surface of the perovskite cell is sequentially stacked with a packaging film and a back glass. PIB butyl glue is used to seal the two sides of the perovskite cell and between the float glass and the back glass. A junction box is provided on the surface of the back glass. Figure 2 As shown, after removing the anti-reflection layer, it is a schematic diagram of the structure of the perovskite photovoltaic module base.
[0039] In one embodiment, before applying the anti-reflection coating liquid, it also includes: preheating the encapsulated perovskite photovoltaic module substrate. The purpose of preheating is to make the coating liquid and glass combine better, which is also conducive to the volatilization of the solvent and film formation. In one embodiment, the preheating treatment specifically includes: heating the encapsulated perovskite photovoltaic module to 40-80°C, such as 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, and then keeping warm for 10-30 minutes, such as 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, etc. Generally, the temperature of the perovskite photovoltaic module is optimal at 45-65°C, and the insulation time is optimal at 15-20 minutes. The heating equipment includes a laminator, a roller press or a separate heating table.
[0040] In one embodiment, after the preheating treatment, the method further comprises: continuously heat treating the encapsulated perovskite photovoltaic module substrate. In one embodiment, the continuous heat treatment maintains the temperature of the encapsulated perovskite photovoltaic module substrate at 40-80°C.
[0041] In one embodiment, the heat source used in the heat treatment includes a roller coating device, that is, the temperature of the working surface of the roller coating device is set to 40-80°C to maintain the surface temperature of the perovskite photovoltaic module after heating. In one embodiment, the roller coating operation can be started when the surface temperature of the perovskite photovoltaic module substrate is between 45°C and 65°C after infrared detection.
[0042] In one embodiment, the anti-reflective coating liquid includes an organosilicon monomer, an alkali catalyst, a template agent and a solvent; wherein the molar number of the organosilicon monomer accounts for 1% to 5% of the total molar number of the anti-reflective coating liquid, the molar number of the alkali catalyst accounts for 1% to 3% of the total molar number of the anti-reflective coating liquid, the molar number of the template agent accounts for 0.1% to 0.5% of the total molar number of the anti-reflective coating liquid, and the molar number of the solvent accounts for 98% to 91.5% of the total molar number of the anti-reflective coating liquid.
[0043] In one embodiment, the molar amount of the organosilicon monomer accounts for 1%, 2%, 3%, 4% or 5% of the total molar amount of the anti-reflection coating solution. When the molar amount of the organosilicon monomer is <1%, the thickness of the generated film layer is insufficient and there is no obvious gain effect; when the molar amount of the organosilicon monomer is >5%, the generated film thickness is too thick and the porosity is reduced, and there is no obvious gain effect. In one embodiment, the organosilicon monomer includes at least one of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, octyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, chloropropyltriethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0044] In one embodiment, the molar amount of the alkali catalyst accounts for 1%, 1.5%, 2%, 2.5% or 3% of the total molar amount of the anti-reflection coating solution. When the molar amount of the alkali catalyst is less than 1%, the catalytic rate is too low and the aging time is too long; when the molar amount of the alkali catalyst is greater than 3%, the catalytic rate is too fast, and silica particles are easily generated and precipitated quickly, resulting in experimental failure. In one embodiment, the alkali catalyst includes at least one of ammonia water, tetramethylammonium hydroxide, sodium hydroxide, potassium hydroxide, acrylamide, ethylenediamine, hexamethylenediamine and triethylamine.
[0045] In one embodiment, the molar amount of the template agent accounts for 0.1%, 0.2%, 0.3%, 0.4% or 0.5% of the total molar amount of the anti-reflective coating solution. When the molar amount of the template agent is <0.1%, too much silica is deposited on the template agent, resulting in an increase in the single size and an increase in the roughness of the film surface; when the molar amount of the template agent is >0.5%, the template agent is excessive and is not completely deposited by silica, the porosity increases, and the mechanical properties of the film layer decrease. In one embodiment, the template agent includes alkyl ammonium bromide. Alkyl ammonium bromide includes at least one of hexadecyl trimethyl ammonium bromide, dodecyl trimethyl ammonium bromide and didodecyl dimethyl ammonium bromide.
[0046] In one embodiment, the molar number of the solvent accounts for 98%, 89%, 90%, 91% or 1.5% of the total molar number of the anti-reflection coating solution. In one embodiment, the solvent includes at least one of ethanol, water, isopropanol, tert-butyl alcohol, ethylene glycol and glycerol.
[0047] Conventional room temperature coating solutions are divided into two types: alkaline and acidic. Alkaline catalytic coating solutions mostly use polyacrylic acid as a template agent, and then add ammonia water as a catalyst. Due to the fast hydrolysis rate and the generally large molecular weight of the polymer, when silica accumulates, the overall template will be relatively large, resulting in larger silica particles, which leads to poor mechanical properties and uneven distribution of the anti-reflection film layer. Conventional acidic catalyst anti-reflection coating solutions use alkylamine template agents and hydrochloric acid as catalysts. Due to the slow hydrolysis of the acidic catalyst, the silica particles formed are small and slowly formed, and the anti-reflection film layer formed is dense, resulting in poor gain effect. The present invention uses an acidic template agent and an alkaline catalyst at the same time, and the corresponding template agent is in a long chain shape. In this way, the film coated after the silicon dioxide is accumulated will be denser than the film layer obtained by the alkaline catalyst template agent due to the acidic template agent, but it will not reach the level of the acidic catalyst, so that it has the advantages of both acid / base catalysis, and has higher porosity and transmittance while ensuring the flatness of the film layer and improving the mechanical strength, and has a good hydrophobic effect, so its gain effect and weather resistance are improved.
[0048] In one embodiment, the method for preparing the anti-reflection coating liquid comprises: mixing an alkali catalyst, a template agent and a solvent to obtain a first mixed solution; dropping an organosilicon monomer into the first mixed solution, and then performing a stirring treatment and an aging treatment. The present invention obtains an anti-reflection coating liquid through a stirring treatment and an aging treatment, which can give the anti-reflection film better mechanical properties, porosity, and transmittance, and can better improve the gain effect and fire resistance of the perovskite photovoltaic module.
[0049] In one embodiment, the stirring treatment time is 2 to 4 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours.
[0050] In one embodiment, the aging treatment time is 20 to 25 hours, such as 20 hours, 21 hours, 22 hours, 23 hours, 24 hours or 25 hours. Before the aging treatment, the container is sealed with a plastic wrap.
[0051] In one embodiment, the coating method includes at least one of roller coating, spray coating and Czochralski method.
[0052] In one embodiment, the coating method is roller coating. Before roller coating, the roller brush is immersed in the anti-reflection coating solution; the immersion time is 30 to 60 seconds, such as 30 seconds, 35 seconds, 40 seconds, 45 seconds, 50 seconds, 55 seconds or 60 seconds. Each time before roller coating the anti-reflection film, the sponge roller brush should be fully immersed once, and the silica AR anti-reflection film coating solution should cover the roller brush. The immersion time is 30 to 60 seconds, so that the roller brush can fully absorb the coating solution.
[0053] In one embodiment, the roller coating pressure is 20-60 N, such as 20 N, 25 N, 28 N, 30 N, 35 N, 40 N, 45 N, 50 N, 55 N or 60 N. The roller brush is pressed on the float glass surface of the perovskite module substrate, and a suitable roller coating pressure is used so that the coating liquid can uniformly overflow from the sponge roller brush during the roller coating process and be evenly coated on the surface of the perovskite photovoltaic module substrate to improve the mechanical properties and porosity of the film layer, and the transmittance gain is high.
[0054] In one embodiment, the moving speed of the roller brush used for roller coating is 200-600 cm / min, for example, 200 cm / min, 250 cm / min, 300 cm / min, 350 cm / min, 400 cm / min, 450 cm / min, 500 cm / min, 550 cm / min or 600 cm / min.
[0055] In one embodiment, the room temperature curing temperature is 18-30°C, such as 18°C, 20°C, 22°C, 25°C, 28°C, 30°C, etc. The room temperature curing time is 5-30min, such as 5min, 10min, 15min, 20min, 25min or 30min, etc. The present invention adopts a suitable room temperature curing time to reduce the influence of the high temperature curing process on the thermal stability of the perovskite battery and improve the battery performance.
[0056] In one embodiment, the washing treatment uses ethanol and / or water. In one embodiment, the glass surface is cleaned with ethanol or water to remove the template, and then cleaned with pure water for 2 to 4 times. Cleaning with ethanol and / or water after encapsulation will not damage the FTO.
[0057] In one embodiment, the drying process comprises air knife drying.
[0058] In one embodiment, the drying process is followed by curing at room temperature for 3 to 7 days.
[0059] According to another aspect of the present invention, the present invention also relates to an anti-reflection film for a perovskite photovoltaic module, which is prepared by the preparation method of the anti-reflection film; the thickness of the anti-reflection film is 80 to 120 nm, for example, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, etc.
[0060] According to another aspect of the present invention, the present invention also relates to a perovskite photovoltaic module, including a perovskite photovoltaic module substrate with the above-mentioned anti-reflection film or the anti-reflection film prepared by the above-mentioned method arranged on the float glass surface of the perovskite photovoltaic module substrate.
[0061] The perovskite photovoltaic module of the present invention has high average light transmittance, large increase in average light transmittance, large short-circuit current density and high conversion efficiency.
[0062] The following is further explained in conjunction with specific embodiments, comparative examples and drawings.
[0063] Example 1
[0064] The method for preparing an anti-reflection film comprises the following steps:
[0065] (1) preheating the encapsulated perovskite photovoltaic module substrate, that is, heating it to 55°C and keeping it warm for 20 minutes; placing the preheated perovskite photovoltaic module substrate on the work surface of the roller coating equipment, and setting the temperature of the work surface to 55°C to maintain the surface temperature of the perovskite photovoltaic module substrate after heating;
[0066] (2) After the surface temperature of the perovskite photovoltaic module substrate is 55°C through infrared detection, the anti-reflection coating liquid is roller-coated on the surface of the float glass of the perovskite photovoltaic module substrate; before roller coating each time, the sponge roller brush should be fully soaked once, and the anti-reflection coating liquid should not exceed the roller brush. The soaking time is 45 seconds, so that the roller brush can fully absorb the coating liquid; the roller coating pressure is 40N, and the moving speed of the roller brush is 400cm / min;
[0067] The preparation method of the anti-reflection coating solution comprises: adding 250 mL (4.282 mol) of ethanol, 20 mL (1.11 mol) of water, 8 g (0.022 mol) of hexadecyltrimethylammonium bromide, and 5 mL (0.13 mol) of ammonia water to a flask in sequence, and stirring evenly until the hexadecyltrimethylammonium bromide is completely dissolved, and then slowly adding 30 mL (0.135 mol) of tetraethoxysilane while stirring, and continuing to stir for 3 hours after the addition is completed, and then sealing with plastic wrap, and continuing to age for 24 hours;
[0068] (3) The roller-coated perovskite photovoltaic module substrate was cured at room temperature for 8 minutes, the glass surface was cleaned with ethanol to remove the template, and then washed with pure water twice and dried with an air knife. The thickness of the obtained anti-reflection film was 100 nm.
[0069] Example 2
[0070] The method for preparing an anti-reflection film comprises the following steps:
[0071] (1) Preheating the encapsulated perovskite photovoltaic module substrate, that is, heating it to 40°C and keeping it warm for 30 minutes; placing the preheated perovskite photovoltaic module substrate on the work surface of the roller coating equipment, and setting the temperature of the work surface to 50°C to maintain the surface temperature of the perovskite photovoltaic module substrate after heating;
[0072] (2) After the surface temperature of the perovskite photovoltaic module substrate is 50°C through infrared detection, the anti-reflection coating liquid is roller-coated on the surface of the float glass of the perovskite photovoltaic module substrate; before roller coating each time, the sponge roller brush should be fully soaked once, and the anti-reflection coating liquid should not exceed the roller brush. The soaking time is 30 seconds, so that the roller brush can fully absorb the coating liquid; the roller coating pressure is 60N, and the moving speed of the roller brush is 200cm / min;
[0073] The preparation method of the anti-reflection coating solution comprises: adding 250 mL (4.282 mol) of ethanol, 20 mL (1.11 mol) of water, 8 g (0.022 mol) of hexadecyltrimethylammonium bromide, and 5 mL (0.13 mol) of ammonia water to a flask in sequence, and stirring evenly until the hexadecyltrimethylammonium bromide is completely dissolved, and then slowly adding 30 mL (0.135 mol) of tetraethoxysilane while stirring, and continuing to stir for 3 hours after the addition is completed, and then sealing with plastic wrap, and continuing to age for 24 hours;
[0074] (3) The roller-coated perovskite photovoltaic module substrate was cured at room temperature for 5 minutes, the glass surface was cleaned with ethanol to remove the template, and then washed with pure water twice and dried with an air knife. The thickness of the obtained anti-reflection film was 120 nm.
[0075] Example 3
[0076] The method for preparing an anti-reflection film comprises the following steps:
[0077] (1) Preheating the encapsulated perovskite photovoltaic module substrate, that is, heating it to 80°C and keeping it warm for 10 minutes; placing the preheated perovskite photovoltaic module substrate on the work surface of the roller coating equipment, and setting the temperature of the work surface to 60°C to maintain the surface temperature of the perovskite photovoltaic module substrate after heating;
[0078] (2) After the surface temperature of the perovskite photovoltaic module substrate is 60° C. through infrared detection, the anti-reflection coating liquid is sprayed onto the surface of the float glass of the perovskite photovoltaic module substrate;
[0079] The preparation method of the anti-reflection coating solution comprises: adding 250 mL (4.282 mol) of ethanol, 20 mL (1.11 mol) of water, 8 g (0.022 mol) of hexadecyltrimethylammonium bromide, and 5 mL (0.13 mol) of ammonia water to a flask in sequence, and stirring evenly until the hexadecyltrimethylammonium bromide is completely dissolved, and then slowly adding 30 mL (0.135 mol) of tetraethoxysilane while stirring, and continuing to stir for 3 hours after the addition is completed, and then sealing with plastic wrap, and continuing to age for 24 hours;
[0080] (3) The sprayed perovskite photovoltaic module substrate was cured at room temperature for 20 minutes, the glass surface was cleaned with ethanol to remove the template, and then washed with pure water twice and dried with an air knife. The thickness of the obtained anti-reflection film was 80 nm.
[0081] Example 4
[0082] A method for preparing an anti-reflection film and a method for preparing an anti-reflection coating solution, comprising: adding 4.3 mol of isopropyl alcohol, 1.2 mol of water, 0.02 mol of dodecyltrimethylammonium bromide, and 0.13 mol of ethylenediamine to a flask in sequence, and stirring evenly until the dodecyltrimethylammonium bromide is completely dissolved, then slowly adding 0.15 mol of dimethyldimethoxysilane while stirring, continuing to stir for 3 hours after the addition is completed, then sealing with a plastic wrap, and continuing to age for 24 hours; other conditions are the same as in Example 1.
[0083] Example 5
[0084] A method for preparing an anti-reflection film and a method for preparing an anti-reflection coating solution, comprising: sequentially adding 4.5 mol of isopropyl alcohol, 1.5 mol of water, 0.02 mol of dodecyltrimethylammonium bromide, 0.01 mol of didodecyldimethylammonium bromide acrylamide, and 0.15 mol of triethylamine into a flask, and stirring evenly until the hexadecyltrimethylammonium bromide is completely dissolved, then slowly and simultaneously adding 0.15 mol of 3-aminopropylmethyldiethoxysilane and 0.15 mol of 3-mercaptopropyltrimethoxysilane while stirring, continuing to stir for 3 hours after the addition is completed, then sealing with a plastic wrap, and continuing to age for 24 hours; other conditions are the same as those in Example 1.
[0085] Comparative Example 1
[0086] The method for preparing an anti-reflection film is the same as that in Example 1 except that step (3) is as follows: curing the roller-coated perovskite photovoltaic module substrate at room temperature for 20 minutes to obtain an anti-reflection film with a thickness of 100 nm; other conditions are the same as those in Example 1.
[0087] Comparative Example 2
[0088] A method for preparing an anti-reflection film, and a method for preparing an anti-reflection coating solution, comprising: adding 3.999 mol of ethanol, 1.11 mol of water, 0.04 mol of hexadecyltrimethylammonium bromide, and 0.13 mol of ammonia water to a flask in sequence, and stirring evenly until the hexadecyltrimethylammonium bromide is completely dissolved, then slowly adding 0.4 mol of tetraethoxysilane while stirring, and continuing to stir for 3 hours after the addition is completed, then sealing with a plastic wrap, and continuing to age for 24 hours; other conditions are the same as in Example 1.
[0089] Experimental example
[0090] The area of the perovskite photovoltaic module in the embodiment and the comparative example is 0.72m 2The perovskite photovoltaic modules obtained in the examples and comparative examples were tested for average light transmittance, short-circuit current, and conversion efficiency. The results are shown in Table 1. The light transmittance was obtained by UV-vis testing; the short-circuit current and conversion efficiency were obtained by testing the battery performance using a solar simulator. The specific testing method is as follows: a steady-state solar simulator was used to test the photoelectric conversion efficiency. Under a standard sunlight of AM1.5G (1000W / m 2 ), set the voltage scanning range to 7.5V to -0.1V, and the scanning rate to 200mV / s. The IU curve and power curve of the perovskite photovoltaic module and the perovskite photovoltaic module substrate of Example 1 of the present invention are as follows Figure 1 shown.
[0091] Table 1 Test results
[0092]
[0093]
[0094] As can be seen from Table 1, the perovskite photovoltaic module obtained by the method of the present invention has a high average light transmittance, a large increase in average light transmittance, a large short-circuit current density, and a high conversion efficiency. Comparative Example 1 was not washed, and the template agent remained. The average light transmittance, average light transmittance increase, short-circuit current density, and conversion efficiency of the perovskite photovoltaic module obtained were relatively low. In the anti-reflection coating solution of Comparative Example 2, the proportion of hexadecyltrimethylammonium bromide and tetraethoxysilane was too high, which affected the film structure of the anti-reflection film. The average light transmittance, average light transmittance increase, short-circuit current density, and conversion efficiency of the perovskite photovoltaic module obtained were relatively low.
[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an anti-reflection film, characterized in that: The following steps are involved: An anti-reflection coating liquid is coated on the glass surface of the encapsulated perovskite photovoltaic module substrate, and then cured at room temperature, washed and dried in sequence.
2. The method for preparing an anti-reflection film according to claim 1, characterized in that: Contains at least one of the following features (1) to (4): (1) Before applying the anti-reflection coating liquid, the method further includes: preheating the encapsulated perovskite photovoltaic module substrate; (2) The preheating treatment specifically includes: heating the packaged perovskite photovoltaic module substrate to 40-80° C. and keeping the temperature for 10-30 minutes; (3) After the preheating treatment, the method further includes: continuously performing heat treatment on the encapsulated perovskite photovoltaic module substrate; (4) The continuous heat treatment maintains the temperature of the encapsulated perovskite photovoltaic module substrate at 40-80°C.
3. The method for preparing an anti-reflection film according to claim 1, characterized in that: The anti-reflection coating solution comprises an organic silicon monomer, an alkali catalyst, a template agent and a solvent; Among them, the molar number of the silicone monomer accounts for 1% to 5% of the total molar number of the anti-reflective coating liquid, the molar number of the alkali catalyst accounts for 1% to 3% of the total molar number of the anti-reflective coating liquid, the molar number of the template agent accounts for 0.1% to 0.5% of the total molar number of the anti-reflective coating liquid, and the molar number of the solvent accounts for 98% to 91.5% of the total molar number of the anti-reflective coating liquid.
4. The method for preparing an anti-reflection film according to claim 3, characterized in that: Contains at least one of the following features (1) to (4): (1) The organosilicon monomer includes at least one of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, octyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, chloropropyltriethoxysilane and 3-mercaptopropyltrimethoxysilane; (2) the alkaline catalyst comprises at least one of ammonia water, tetramethylammonium hydroxide, sodium hydroxide, potassium hydroxide, acrylamide, ethylenediamine, hexamethylenediamine and triethylamine; (3) The template comprises alkylammonium bromide; (4) The solvent includes at least one of ethanol, water, isopropanol, tert-butyl alcohol, ethylene glycol and glycerol.
5. The method for preparing an anti-reflection film according to claim 3, characterized in that: Contains at least one of the following features (1) to (3): (1) The method for preparing the anti-reflection coating solution comprises: mixing an alkali catalyst, a template agent and a solvent to obtain a first mixed solution; adding an organosilicon monomer dropwise to the first mixed solution, and then performing stirring and aging treatments; (2) The stirring treatment time is 2 to 4 hours; (3) The aging treatment time is 20 to 25 hours.
6. The method for preparing an anti-reflection film according to claim 1, characterized in that: The coating method includes at least one of roller coating, spray coating and Czochralski coating.
7. The method for preparing an anti-reflection film according to claim 1, characterized in that: The room temperature curing temperature is 18 to 30° C., and the room temperature curing time is 5 to 30 minutes.
8. The method for preparing an anti-reflection film according to claim 1, characterized in that: The washing treatment uses ethanol and / or water.
9. An anti-reflection film, characterized in that: The anti-reflection film is prepared by the method for preparing the anti-reflection film according to any one of claims 1 to 8; the thickness of the anti-reflection film is 80 to 120 nm.
10. A perovskite photovoltaic module, characterized in that: The invention comprises a perovskite photovoltaic module substrate and an anti-reflection film arranged on the float glass surface of the perovskite photovoltaic module substrate; the anti-reflection film is the anti-reflection film according to claim 9 or an anti-reflection film prepared by the preparation method of the anti-reflection film according to any one of claims 1 to 8.
Citation Information
Patent Citations
SiO2 antireflection thin film and preparation method thereof
CN102617045A
Preparation method of self-curing antireflection coating on glass surface
CN104310792A
Double-layer coated photovoltaic glass and production method and production line thereof
CN114409271A
Apparatus and method for measuring bone to implant contact ratio
KR1020210001076A