Resin composition and automotive member

By adding chemical adsorbent to the resin composition to capture volatile organic compounds, the problems of odor and atomization during the forming process of biomass filler are solved, and the environmental safety and product quality of the forming process are improved.

CN119072524APending Publication Date: 2024-12-03INOAC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380035656.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-01-20
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When forming using a resin composition containing a filler derived from biomass, it is difficult to completely suppress the generation of odor and the atomization problems caused by this, and the prior art is difficult to completely solve the problem by reducing the forming temperature alone.

Method used

The filler derived from biomass is dispersed in the olefin-based thermoplastic resin and/or thermoplastic elastomer, and a chemical adsorbent is added to capture volatile organic compounds, inhibiting the generation of odor and atomization.

Benefits of technology

Through the use of chemical adsorbents, the generated volatile organic compounds are effectively captured, the generation of odor and atomization is inhibited, and the environmental safety and product quality of the forming process are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005096095940000101
    Figure BDA0005096095940000101
  • Figure BDA0005096095940000131
    Figure BDA0005096095940000131
Patent Text Reader

Abstract

The resin composition comprises: an olefin-based thermoplastic resin and / or a thermoplastic elastomer; a filler derived from biomass; and a chemical adsorbent for chemically adsorbing volatile organic compounds (VOCs) generated from the filler. The average particle diameter of the filler is preferably 1 [mu] m or more and 500 [mu] m or less. It is preferable that the content of the filler is more than 0 mass% and 60 mass% or less. The content of the chemical adsorbent is preferably from 0.1 mass% to 15 mass% (inclusive). The automotive member is provided with the resin composition according to the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition and an automobile component, and more particularly to a resin composition in which a biomass-derived filler is dispersed in an olefin-based thermoplastic resin and / or a thermoplastic elastomer, and an automobile component having the resin composition. Background Art

[0002] Olefin thermoplastic resins represented by polypropylene are used for various purposes due to their excellent strength, impact resistance, heat resistance, etc. In particular, filler-reinforced polypropylene (PPF), in which fillers are dispersed in polypropylene, is used as a material for automotive interior parts due to its high rigidity and excellent impact resistance. Filler-reinforced plastics such as PPF are usually produced by molding a mixture of resin and filler at high temperature.

[0003] In recent years, in order to protect the global environment, sustainable development is needed. In filler reinforced plastics, it is not only resins, but also fillers that wish to utilize biomass resources. As fillers derived from biomass, for example, there are scallop shells, eggshells, trees, pulp, bamboo, bagasse, and rice husks. However, when the filler derived from biomass is mixed with the resin at high temperature at the same time, a significant odor will be generated from the filler derived from biomass (particularly a filler containing cellulose), causing the working environment to deteriorate.

[0004] Therefore, various proposals have been made in the past to solve this problem.

[0005] For example, Patent Document 1 discloses a polypropylene resin composition comprising a polypropylene resin (A) having a melting point of 150° C. or higher, a polypropylene resin (B) having a melting point of 110° C. or higher and lower than 150° C., and a biomass material (C).

[0006] The same patent document states:

[0007] (a) by setting the melting point of the polypropylene resin (B) to be lower than 150° C., the temperature at which the polypropylene resin composition is molded can be relatively low; and

[0008] (b) This can suppress the generation of odor and ensure moldability and product quality.

[0009] Patent Document 1 states that when a filler-reinforced resin containing a filler derived from biomass is molded, the generation of odor can be suppressed by lowering the molding temperature. However, it is difficult to completely suppress the generation of odor simply by lowering the molding temperature. In addition, even after molding, odor components may be generated from the molded body, causing atomization.

[0010] Prior art documents

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2021-050270 Summary of the invention

[0013] Problems to be solved by the invention

[0014] An object of the present invention is to suppress the generation of odor and fogging caused by the odor in a resin composition containing a biomass-derived filler.

[0015] Another problem to be solved by the present invention is to provide an automobile component comprising such a resin composition.

[0016] Means of solving problems

[0017] In order to solve the above problems, the resin composition according to the present invention comprises:

[0018] Olefin thermoplastic resin and / or thermoplastic elastomer;

[0019] Fillers derived from biomass; and

[0020] A chemical adsorbent is used to chemically adsorb volatile organic compounds (VOC) generated from the filler.

[0021] The automobile member according to the present invention comprises the resin composition according to the present invention.

[0022] Effects of the Invention

[0023] When a filler derived from biomass is dispersed in an olefin-based thermoplastic resin and / or a thermoplastic elastomer, if a chemical adsorbent is further added to the raw material, even if volatile organic compounds (VOCs) are generated from the raw material or the molded body after heating, the chemical adsorbent captures the VOCs. As a result, the generation of odors caused by the VOCs and the misting caused by the odors can be suppressed. DETAILED DESCRIPTION

[0024] Hereinafter, one embodiment of the present invention will be described in detail.

[0025] [1. Resin composition]

[0026] The resin composition involved in the present invention comprises:

[0027] Olefin thermoplastic resin and / or thermoplastic elastomer;

[0028] Fillers derived from biomass; and

[0029] A chemical adsorbent is used to chemically adsorb volatile organic compounds (VOC) generated from the filler.

[0030] [1.1. Main ingredients]

[0031] [1.1.1. Olefin thermoplastic resin and thermoplastic elastomer]

[0032] The matrix of the resin composition is composed of an olefinic thermoplastic resin and / or a thermoplastic elastomer. The resin composition may contain either an olefinic thermoplastic resin or a thermoplastic elastomer, or may contain both.

[0033] In the present invention, the types of olefin thermoplastic resins and thermoplastic elastomers are not particularly limited, and the most suitable material can be selected according to the purpose. As olefin thermoplastic resins and thermoplastic elastomers, specifically, there are the following substances. The resin composition may be a substance containing any one of the following olefin thermoplastic resins or thermoplastic elastomers, or may be a substance containing two or more olefin thermoplastic resins or thermoplastic elastomers.

[0034] Furthermore, the olefin-based thermoplastic resin and thermoplastic elastomer described below may be synthesized using olefins derived from fossil fuels as raw materials, or may be synthesized using olefins derived from biomass as raw materials.

[0035] [1.1.1.1. Specific examples of olefin-based thermoplastic resins]

[0036] (A) Polyethylene resin:

[0037] Examples of polyethylene resins include:

[0038] (a) High-density polyethylene,

[0039] (b) linear low density polyethylene, and

[0040] (c) Low-density polyethylene

[0041] wait.

[0042] Linear low-density polyethylene is obtained by copolymerizing ethylene with a small amount of α-olefins, such as propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-heptene, and 1-octene.

[0043] (B) Polypropylene resin:

[0044] Examples of polypropylene resins include:

[0045] (a) Homopolypropylene (H-PP);

[0046] (b) block polypropylene (B-PP) having a compatibilizer (e.g., ethylene-propylene rubber (EPR)) present at the interface between H-PP and polyethylene (PE); and

[0047] (c) Propylene-α-olefin copolymer (R-PP)

[0048] wait.

[0049] Examples of the α-olefin constituting the propylene-α-olefin copolymer include ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene.

[0050] (C) Ethylene-vinyl acetate copolymer.

[0051] Ethylene-vinyl acetate copolymer (EVA) is a copolymer of ethylene and vinyl acetate. The content of vinyl acetate in EVA is usually 10-40 mass%.

[0052] [1.1.1.2. Specific examples of thermoplastic elastomers]

[0053] (D) Olefin thermoplastic elastomer:

[0054] Examples of olefin-based thermoplastic elastomers include:

[0055] (a) copolymers of ethylene and α-olefins having 3 to 20 carbon atoms;

[0056] (b) copolymers of ethylene with α-olefins having 3 to 20 carbon atoms and cyclic olefins;

[0057] (c) Ethylene copolymers using various vinyl compounds such as styrene, vinyl acetate, (meth)acrylic acid, (meth)acrylates as comonomers;

[0058] (d) copolymers of propylene and α-olefins having 4 to 20 carbon atoms;

[0059] (e) copolymers of propylene with α-olefins having 4 to 20 carbon atoms and cyclic olefins;

[0060] (f) Propylene copolymers using various vinyl compounds such as styrene, vinyl acetate, (meth)acrylic acid, (meth)acrylates as comonomers;

[0061] (g) A mixture of at least one substance selected from the group consisting of polyethylene and polypropylene and at least one substance selected from the group consisting of polybutadiene, hydrogenated polybutadiene, polyisoprene, hydrogenated polyisoprene, polyisobutylene, ethylene-propylene copolymer, ethylene-propylene-diene copolymer, ethylene-butylene copolymer, hydrogenated styrene butadiene, and α-olefin copolymer

[0062] wait.

[0063] When the olefinic thermoplastic elastomer is a copolymer, the copolymerization form may be either block copolymerization or graft copolymerization.

[0064] In addition, the olefin-based thermoplastic elastomer may be modified with at least one functional group selected from the group consisting of anhydride groups, carboxyl groups, amino groups, imino groups, alkoxysilyl groups, silanol groups, silyl ether groups, hydroxyl groups, and epoxy groups.

[0065] (E) Styrene thermoplastic elastomer:

[0066] Styrene-based thermoplastic elastomers are block copolymers having a block of a polymer or copolymer of styrene and a block of a polymer or copolymer of a conjugated diene compound. As conjugated diene compounds, for example, isoprene and butadiene are provided. In addition, styrene-based thermoplastic elastomers may be substances hydrogenated at double bond portions.

[0067] Examples of styrene-based thermoplastic elastomers include:

[0068] (a) styrene-isoprene block copolymer,

[0069] (b) styrene-isoprene-styrene block copolymer,

[0070] (c) styrene-butadiene block copolymer,

[0071] (d) styrene-butadiene-styrene block copolymer,

[0072] (e) styrene-ethylene / butylene-styrene block copolymer (SEBS),

[0073] (f) styrene-ethylene / propylene-styrene block copolymer (SEPS),

[0074] (g) styrene-ethylene / butylene block copolymer (SEB),

[0075] (h) styrene-ethylene / propylene block copolymer (SEP), and

[0076] (i) Styrene-ethylene / butylene-crystalline olefin block copolymer (SEBC)

[0077] wait.

[0078] (F) Vinyl chloride thermoplastic elastomer:

[0079] The vinyl chloride-based thermoplastic elastomer is an elastomer in which both the hard segment and the soft segment include polyvinyl chloride.

[0080] (G) Polyurethane thermoplastic elastomer:

[0081] Polyurethane thermoplastic elastomers are elastomers whose hard segments include polyurethane and whose soft segments include polyether, polyester, etc.

[0082] (H) Polyester thermoplastic elastomer:

[0083] The polyester-based thermoplastic elastomer is an elastomer whose hard segment includes polyester and whose soft segment includes polyether.

[0084] (I) Polyamide thermoplastic elastomer:

[0085] The polyamide-based thermoplastic elastomer is an elastomer whose hard segment includes polyamide and whose soft segment includes polypropylene glycol (PPG), polytetramethylene glycol (PTMG) and the like.

[0086] [1.1.2.Padding]

[0087] [A. Materials]

[0088] The filler is dispersed in a matrix including an olefinic thermoplastic resin and / or a thermoplastic elastomer. In the present invention, "filler" refers to a filler derived from biomass.

[0089] The filler is particularly preferably a filler containing cellulose, in other words, the filler is particularly preferably a filler derived from a plant (derived from lignocellulosic biomass or derived from cellulose biomass). As a filler containing cellulose, specifically, there are the following substances. The resin composition can be a substance containing any one of the following fillers, or can also be a substance containing two or more fillers.

[0090] Examples of fillers derived from cellulosic biomass include:

[0091] (a) α-fiber flocs obtained by alkali treating wood pulp and mechanically chopping it;

[0092] (b) Cotton linters and cotton wool obtained from cotton seeds; and

[0093] (c) Artificial floccules obtained by shredding rayon

[0094] wait.

[0095] As fillers derived from lignocellulosic biomass there are, for example:

[0096] (a) Wood pulp, refined graft pulp (RGP), paper pulp, and waste paper;

[0097] (b) Wood chips after pulverization;

[0098] (c) wood flour, including crushed materials, sawdust, shavings, etc. of pine, fir, poplar, bamboo, bagasse, oil palm trunks, etc.;

[0099] (d) husk powder, which includes crushed fruit such as walnuts, peanuts, coconuts, etc.; and

[0100] (e) Rice husk powder

[0101] wait.

[0102] In addition, fillers can also be derived from:

[0103] (a) esterified cellulose biomass having polybasic acid anhydride added to the hydroxyl groups of the cellulose biomass,

[0104] (b) esterified lignocellulosic biomass with polyacid anhydride added to the hydroxyl groups of lignocellulosic biomass,

[0105] (c) oligoesterified cellulose biomass to which polyacid anhydride and monoepoxy compound are added to hydroxyl groups of cellulose biomass;

[0106] (d) oligoesterified lignocellulosic biomass to which polyacid anhydride and monoepoxy compound are added to hydroxyl groups of lignocellulosic biomass;

[0107] (e) oligoesterified cellulose biomass to which polyacid anhydride and polyol are added to hydroxyl groups of cellulose biomass; or

[0108] (f) Adding oligoesters of polyanhydrides and polyols to the hydroxyl groups of the lignocellulosic biomass

[0109] of substance.

[0110] [B. Shape]

[0111] In the present invention, the shape of the filler is not particularly limited, and the most appropriate shape can be selected according to the purpose. Examples of the shape of the filler include spherical, needle-like, and plate-like shapes.

[0112] [C. Average particle size]

[0113] The average particle size of the filler is the median particle size (D 50 ).

[0114] In the present invention, the average particle size of the filler is not particularly limited, and an optimal value can be selected depending on the purpose.

[0115] Generally, if the average particle size of the filler is too small, it is difficult to uniformly disperse the filler. Therefore, the average particle size of the filler is preferably 1 μm or more. The average particle size is more preferably 5 μm or more, and further preferably 10 μm or more.

[0116] On the other hand, if the average particle size of the filler is too large, the mechanical properties of the resin composition may be reduced. Therefore, the average particle size of the filler is preferably 500 μm or less. The average particle size is more preferably 350 μm or less, and further preferably 200 μm or less.

[0117] [1.1.3. Chemical adsorbent]

[0118] "Chemical adsorbent" refers to a compound (additive) that has the following reactivity when the resin composition or the raw material mixture used to produce the resin composition is heated, irradiated with light, etc.: it can chemically adsorb volatile organic compounds (VOC) mainly generated from fillers. Examples of VOCs include aldehydes, ketones, and carboxylic acids. Specifically, the following substances are included as chemical adsorbents. The resin composition may be a substance containing any one of the following chemical adsorbents, or may be a substance containing two or more chemical adsorbents.

[0119] (A) A chemical adsorbent comprising an organic compound having an amino group or an amide group:

[0120] Examples of the chemical adsorbent including an organic compound having an amino group include alkylamine, tetramethylenediamine, ethanolamine, piperidine, and the like.

[0121] Examples of the chemical adsorbent including a compound having an amide group include 2-acrylamido-2-methylpropanesulfonic acid and the like.

[0122] (B) Chemical adsorbents comprising basic inorganic compounds:

[0123] As chemical adsorbents including basic inorganic compounds, there are, for example:

[0124] (a) Hydroxides such as sodium hydroxide, calcium hydroxide, potassium hydroxide, magnesium hydroxide and ferric hydroxide;

[0125] (b) basic oxides such as sodium oxide, magnesium oxide, and calcium oxide; and

[0126] (c) Carbonates or bicarbonates such as sodium carbonate, sodium bicarbonate, and calcium carbonate

[0127] wait.

[0128] Among them, calcium oxide is suitable as a chemical adsorbent because of its excellent adsorption effect on VOCs and glass fogging components. For example, when aldehydes are oxidized to carboxylic acids by heat or light, calcium oxide quickly adsorbs the carboxylic acids. Calcium oxide can be a mineral-derived substance or a biological-derived substance (for example, a scallop shell or eggshell fired product).

[0129] Among fillers, wood powder has a high hygroscopicity, so when heated, it may easily cause oil decomposition and higher fatty acids to be released. It is believed that due to this influence, the oil decomposition products will volatilize. On the contrary, if calcium oxide is further added to the resin composition containing wood powder as a filler, the calcium oxide will chemically adsorb the oil decomposition products. As a result, it is believed that odor and glass fogging are suppressed.

[0130] The chemical adsorbent may be directly added to the resin composition, or the chemical adsorbent may be supported on the surface of an inorganic porous body and then added to the resin composition.

[0131] The inorganic porous body is not particularly limited as long as it is an inorganic compound having a plurality of pores on its surface. Examples of the material of the inorganic porous body include zeolite, silicon dioxide, activated carbon, titanium dioxide, calcium phosphate, aluminum oxide, aluminum hydroxide, magnesium hydroxide, etc. In addition, examples of the shape of the inorganic porous body include spherical, rod-shaped, elliptical, etc.

[0132] [1.2. Sub-components]

[0133] The resin composition of the present invention may be composed only of the above-mentioned main component and inevitable impurities, or may contain various secondary components in addition to these. The secondary components include the following.

[0134] [1.2.1. Compatibilizer]

[0135] The resin composition according to the present invention may contain a compatibilizer.

[0136] "Compatibilizer" refers to an additive used to make olefin thermoplastic resin and / or thermoplastic elastomer compatible with filler. In the present invention, there is no particular limitation on the compatibilizer as long as it can achieve such a function. As compatibilizers, specifically, there are the following substances. The resin composition may be a substance containing any one of these compatibilizers, or may be a substance containing two or more compatibilizers.

[0137] (A) Saturated carboxylic acid compatibilizer:

[0138] Examples of the saturated carboxylic acid-based compatibilizer include saturated carboxylic acids and derivatives of saturated carboxylic acids.

[0139] Examples of the saturated carboxylic acid include succinic anhydride, succinic acid, phthalic anhydride, phthalic acid, tetrahydrophthalic anhydride, and adipic anhydride.

[0140] Examples of the derivatives of saturated carboxylic acids include metal salts, amides, imides, and esters of saturated carboxylic acids.

[0141] (B) Unsaturated carboxylic acid compatibilizer:

[0142] Examples of the unsaturated carboxylic acid-based compatibilizer include unsaturated carboxylic acids, derivatives of unsaturated carboxylic acids, and olefin-based thermoplastic resins modified with unsaturated carboxylic acids or derivatives thereof.

[0143] Examples of the unsaturated carboxylic acid include maleic anhydride, maleic acid, nadic anhydride, itaconic anhydride, itaconic acid, citraconic anhydride, citraconic acid, crotonic acid, isocrotonic acid, mesaconic acid, angelica acid, sorbic acid, and acrylic acid.

[0144] Examples of the derivative of the unsaturated carboxylic acid include metal salts, amides, imides, and esters of the unsaturated carboxylic acid.

[0145] [1.2.2. Antioxidants]

[0146] The resin composition according to the present invention may contain an antioxidant.

[0147] "Antioxidant" refers to an additive used to inhibit the oxidation of the resin composition caused by free radicals. Examples of antioxidants include phenolic antioxidants that have the function of capturing free radicals and phosphorus antioxidants that have the function of decomposing hydrogen peroxide. The resin composition of the present invention may contain any one of these antioxidants, or may contain two or more antioxidants.

[0148] [1.2.3. Weathering agent]

[0149] The resin composition according to the present invention may contain a weathering agent.

[0150] "Weathering agent" refers to an additive used to inhibit the degradation of the resin composition caused by outdoor natural environments such as sunlight, temperature, humidity, and rain. Examples of weathering agents include ultraviolet absorbers for absorbing ultraviolet rays and light stabilizers for stabilizing free radicals generated by ultraviolet rays. The resin composition of the present invention may contain any one of these weathering agents, or may contain two or more weathering agents.

[0151] [1.2.4. Other secondary components]

[0152] The resin composition according to the present invention may further contain auxiliary components other than those mentioned above.

[0153] As other secondary components, for example, there are nucleating agents, heat stabilizers, antistatic agents, slip agents, anti-blocking agents, antifogging agents, neutralizers, metal deactivators, surfactants, colorants, antibacterial / mildewproof agents, flame retardants, plasticizers, dispersants, fillers, foaming agents, crosslinking agents, conductive agents, preservatives, fragrances, deodorants, and insect repellents, etc. The resin composition can be a material further containing any one of these secondary components, or can also be a material further containing two or more.

[0154] [1.3. Composition]

[0155] [1.3.1. Filler content]

[0156] The resin composition according to the present invention preferably satisfies the following formula (1).

[0157] 0<X≤60mass%…(1)

[0158] Here, X (mass %) is the ratio of the mass of the filler to the total mass of the resin composition.

[0159] Generally, if X is too small, mechanical properties may be reduced. Therefore, X is preferably greater than 0. X is more preferably 5 mass% or more, and further preferably 10 mass% or more.

[0160] On the other hand, if X is too large, it is difficult to uniformly disperse the filler in the olefinic thermoplastic resin and / or the thermoplastic elastomer. Therefore, X is preferably 60 mass% or less. More preferably, X is 50% or less, 40% or less, or 30% or less.

[0161] [1.3.2. Content of chemical adsorbent]

[0162] The resin composition according to the present invention preferably satisfies the following formula (2).

[0163] 0.1≤Y≤15mass%…(2)

[0164] Here, Y (mass %) is the ratio of the mass of the chemical adsorbent to the total mass of the resin composition.

[0165] If Y is too small, it may be difficult to suppress the generation of odor and atomization. Therefore, Y is preferably 0.1 mass% or more. More preferably, Y is 0.3 mass% or more, 0.5 mass% or more, or 1.0 mass% or more.

[0166] On the other hand, if Y is too large, not only will the effect as a chemical adsorbent be saturated, but the mechanical properties will also be reduced. Therefore, Y is preferably 15 mass% or less. More preferably, Y is 10 mass% or less, 9 mass% or less, 8 mass% or less, 7 mass% or less, 6 mass% or less, 5 mass% or less, 4 mass% or less, or 3 mass% or less.

[0167] [1.3.2. Content of accessory ingredients]

[0168] The resin composition of the present invention may contain a filler and a chemical adsorbent, and the rest may include an olefinic thermoplastic resin and / or a thermoplastic elastomer, and inevitable impurities. Alternatively, the resin composition of the present invention may contain a filler, a chemical adsorbent, and one or more secondary components, and the rest may include an olefinic thermoplastic resin and / or a thermoplastic elastomer, and inevitable impurities.

[0169] When the resin composition contains an accessory component, the content of the accessory component is not particularly limited, and the most appropriate content can be selected according to the purpose.

[0170] [1.4.Purpose]

[0171] The resin composition of the present invention can be used for various purposes. For example, the resin composition of the present invention can be used for:

[0172] (a) Automobile components,

[0173] (b) pellets for producing raw materials for injection molded products, and

[0174] (c) Masterbatch containing fillers dispersed at high concentrations

[0175] wait.

[0176] Examples of automobile parts including the resin composition according to the present invention include:

[0177] (a-1) Interior components such as instrument panels, trims, covers, pillars, and engine hoods; and

[0178] (a-2) Exterior components such as bumpers, moldings, fenders, wheel covers, weatherstrips, glass runners, wipers, etc.

[0179] wait.

[0180] [2. Method for producing resin composition]

[0181] The resin composition involved in the present invention is obtained by the following method:

[0182] (a) preparing the main component and, if necessary, the auxiliary components in a predetermined ratio,

[0183] (b) Kneading the raw material mixture while heating it at a predetermined temperature, and molding the kneaded product into a predetermined shape.

[0184] The heating temperature of the raw materials is not particularly limited, and the most suitable temperature can be selected according to the purpose. Generally, the higher the heating temperature, the easier it is to evenly disperse the filler. On the other hand, if the heating temperature is too high, the resin may change color, or volatile organic compounds (VOC) may be easily generated from the filler. In order to suppress the discoloration of the resin and the generation of VOC, the heating temperature is preferably below 200°C.

[0185] [3. Function]

[0186] When a filler derived from biomass is dispersed in an olefin-based thermoplastic resin and / or a thermoplastic elastomer, if a chemical adsorbent is further added to the raw material, even if volatile organic compounds (VOCs) are generated from the raw material or the molded body after heating, the chemical adsorbent captures the VOCs. As a result, the generation of odors caused by the VOCs and the misting caused by the odors can be suppressed.

[0187] Example

[0188] (Examples 1 to 5, Comparative Examples 1 to 3, Reference Examples 1 to 3)

[0189] [1. Sample preparation]

[0190] The raw materials shown in Table 1 were prepared in the ratios shown in Table 1 to obtain a raw material mixture. The raw material mixture was melt-kneaded using a twin-screw extruder to prepare pellets. The molding temperature was set to 170°C.

[0191] Next, the pellets were put into an injection molding machine to perform injection molding of a test piece material. The injection molding temperature was set at 180° C. Test pieces of a predetermined size were cut out from the obtained test piece material and various tests were performed.

[0192] It should be noted that block polypropylene (B-PP) (BC04ASW, manufactured by Japan Polypropylene Co., Ltd.) was used as the olefin-based thermoplastic resin, and ethylene octene rubber (EOR) (ENGAGE 8180, manufactured by Dow Chemical Japan Co., Ltd.) was used as the thermoplastic elastomer.

[0193] In the filling, used:

[0194] (a) Wood powder having an average particle size of 70 to 150 μm (Examples 1 to 2, Comparative Examples 1 to 3) (ARBOCEL C-100 manufactured by Reten Mine Japan Co., Ltd.),

[0195] (b) Wood powder having an average particle size of 20 to 40 μm (Examples 3 to 5) (ARBOCEL CW630PU manufactured by Reten Mine Japan Co., Ltd.), or

[0196] (c) Talc (Reference Example 1) (SK-7800, manufactured by Kaijo Corporation).

[0197] As the compatibilizer, maleic anhydride-modified polypropylene (PRIEX 20097, manufactured by Big Chem Japan Co., Ltd.) was used.

[0198] Among the chemical adsorbents used:

[0199] (a) CaO-based chemical adsorbent (BYK-MAX OR 4206, manufactured by BYK Chemi Japan Co., Ltd., CaO content: 10 to 20%),

[0200] (b) CaO-based chemical adsorbent (RECYCLOBYK 4371 manufactured by Bick Chemie Japan Co., Ltd., CaO content: 30 to 40%), or

[0201] (c) Amine chemical adsorbent (manufactured by Otsuka Chemical Co., Ltd., H-6000HS).

[0202] In addition, as other additives, used:

[0203] (a) phenolic antioxidant (manufactured by ADEKA Corporation, AO-60),

[0204] (b) a phosphorus antioxidant (manufactured by ADEKA Corporation, 2112), and

[0205] (c) Weathering agent (manufactured by BASF Corporation, XT-855).

[0206] [Table 1]

[0207]

[0208] [2. Test method]

[0209] [2.1. Mechanical properties]

[0210] [2.1.1. Specific gravity]

[0211] According to JIS K 7112, the specific gravity of the test piece was measured.

[0212] [2.1.2. Bending strength]

[0213] Flexural strength and elastic modulus were measured according to ISO 178.

[0214] It should be noted that the bending strength is preferably 20 MPa or more. The bending strength is more preferably 23 MPa or more, and further preferably 25 MPa or more. The upper limit of the bending strength is not particularly limited, but is usually 80 MPa or less.

[0215] The flexural modulus is preferably 1000 MPa or more. The flexural modulus is more preferably 1200 MPa or more, and further preferably 1400 MPa or more. The upper limit of the flexural modulus is not particularly limited, but is usually 8000 MPa or less.

[0216] [2.1.3. Impact value]

[0217] Charpy impact test was performed according to ISO 179 / 1eA. The test conditions were set to 23°C·notched or -30°C·notched.

[0218] It should be noted that the impact value at 23°C is preferably 2.0 kJ / m 2 The impact value at 23°C is more preferably 3.0 kJ / m 2 More preferably, 5.0 kJ / m 2 The greater the impact value at 23°C, the better.

[0219] In addition, the impact value at -30°C is preferably 1.2 kJ / m 2 The impact value at -30°C is more preferably 1.5 kJ / m 2 More preferably, 2.0 kJ / m 2 The greater the impact value at -30°C, the better.

[0220] [2.1.4. Load deflection temperature (HDT)]

[0221] The load deflection temperature (HDT) was measured according to ISO 75-2. The bending stress (load) was set to 0.45 MPa.

[0222] It should be noted that the HDT is preferably 90° C. or higher. The HDT is more preferably 100° C. or higher, and further preferably 110° C. or higher. The upper limit of the HDT is not particularly limited, but is usually 200° C. or lower.

[0223] [2.2. Odor characteristics]

[0224] [2.2.1.VOC]

[0225] The measurement of volatile organic compounds (VOC) was carried out under indoor conditions of temperature: 23±2°C, humidity: 50±5%RH. The analysis was carried out within 14 days after the preparation of the test piece.

[0226] Fill a 10L Tedlar (registered trademark) sampling bag three times with pure nitrogen to replace the gas in the sampling bag. Put a test piece (100mm×80mm×t2mm) into the sampling bag and seal it. After heating the sampling bag at 65°C for 2 hours using a hot air dryer, the volatile components in the sampling bag are adsorbed on silica gel. In addition, the volatile components adsorbed on the silica gel are extracted with a solvent and analyzed by high performance liquid chromatography (HPLC). The total amount of volatile components (aldehydes) is measured by comparison with a standard sample.

[0227] It should be noted that, when the VOC is HCHO, the volatilization amount is preferably 1.0 μg / unit or less. The volatilization amount is more preferably 0.5 μg / unit or less, and further preferably 0.1 μg / unit or less. The smaller the HCHO volatilization amount, the better.

[0228] When the VOC is CH3CHO, the volatilization amount is preferably 1.6 μg / unit or less. The volatilization amount is more preferably 1.0 μg / unit or less, and further preferably 0.5 μg / unit or less. The smaller the volatilization amount of CH3CHO, the better.

[0229] [2.2.2. Glass fogging (fogging)]

[0230] The glass fogging was measured at room temperature of 23°C ± 2°C and 50 ± 5% RH. The analysis was performed within 14 days after the test piece was prepared.

[0231] A glass plate of □47mm×t3mm (glass haze ≤ 0.5%) was used as the glass plate. The test pieces (a total of 2 pieces of 100mm×25mm×t2mm) were placed in a glass bottle and covered with a glass plate. In this state, the glass bottle was heated in an oil bath at 80±2°C for 20 hours. One hour after the test, the glass haze (%) of the glass plate was measured using an integrating sphere transmittance measuring device.

[0232] It should be noted that the glass fogging is preferably 5% or less. The glass fogging is more preferably 3% or less, and further preferably 1.5% or less. The smaller the glass fogging, the better.

[0233] [3. Results]

[0234] [3.1. Mechanical properties]

[0235] The results are shown in Table 2. From Table 2, the following can be seen.

[0236] (1) Reference Example 1 had good mechanical properties and odor characteristics, but the specific gravity exceeded 1.0. This is considered to be due to the use of talc as a filler.

[0237] (2) Reference Examples 2 and 3 have good odor properties, but the elastic modulus is less than 1400 MPa, and the load deformation temperature is also reduced to less than 100°C. This is believed to be due to the absence of filler. In addition, the bending strength of Reference Example 3 is reduced to less than 25 MPa. This is believed to be due to the increase in the amount of elastomer.

[0238] (3) In Comparative Example 1, the bending strength was 25 MPa or more, the elastic modulus was 1400 MPa or more, and the impact value at -30°C was 2.0 kJ / m 2 However, in Comparative Example 1, the impact value at room temperature was reduced to less than 5 kJ / m 2 This is believed to be due to the filler not being evenly dispersed due to the absence of a compatibilizer.

[0239] In Comparative Example 1, the amount of CH3CHO volatilization exceeded 1.60 μg / glass, and the glass haze exceeded 5%. This is believed to be due to the absence of a chemical adsorbent.

[0240] (4) Comparative Examples 2 and 3 have good mechanical properties because they contain fillers and compatibilizers. However, the odor characteristics of Comparative Examples 2 and 3 deteriorate. In particular, in Comparative Example 2, the HCHO volatilization amount exceeds 1.00 μg / piece. This is believed to be due to the absence of a chemical adsorbent.

[0241] (5) Fourier transform infrared spectrophotometer (FT-IR) was used to analyze the components adhering to the glass plate during the glass fogging test of Comparative Examples 1 to 3. The results showed that the main cause of glass fogging in Comparative Examples 1 to 3 was fatty acid ester.

[0242] (6) The mechanical properties and odor characteristics of Examples 1 to 5 are good. However, in Examples 3 to 5, the specific gravity exceeds 1.0. This is due to the large amount of wood powder formulated.

[0243] (7) The more CaO is added, the more CH3CHO is generated. In addition, if CaO and amine chemical adsorbents are used simultaneously, the generation of CH3CHO is further suppressed.

[0244] [Table 2]

[0245]

[0246] As mentioned above, although embodiment of this invention is described in detail, this invention is not limited to the said embodiment, Various changes can be made within the range which does not deviate from the summary of this invention.

[0247] Industrial Applicability

[0248] The resin composition of the present invention can be used for injection molded articles, pellets as a raw material for producing injection molded articles, and master batches in which fillers are dispersed at a high concentration.

Claims

1. A resin composition, wherein The resin composition comprises: Olefin thermoplastic resin and / or thermoplastic elastomer; Fillers derived from biomass; and A chemical adsorbent is used to chemically adsorb volatile organic compounds (VOC) generated from the filler.

2. The resin composition according to claim 1, wherein The average particle size of the filler is 1 μm or more and 500 μm or less.

3. The resin composition according to claim 1 or 2, wherein The resin composition satisfies the following formula (1): 0<X≤60mass%…(1) Here, X (mass %) is the ratio of the mass of the filler to the total mass of the resin composition.

4. The resin composition according to claim 1 or 2, wherein The resin composition satisfies the following formula (2): 0.1≤Y≤15mass%…(2) Here, Y (mass %) is the ratio of the mass of the chemical adsorbent to the total mass of the resin composition.

5. A component for an automobile, wherein: The automotive member comprises the resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polypropylene resin composition

    JP2021050270A