Positive electrode and lithium secondary battery manufactured using same

By using a combination of lithium transition metal phosphate and fluorine-containing adhesive in the positive electrode of lithium secondary battery, the porosity and adhesive molecular weight are adjusted, and the problems of insufficient positive electrode cracks and adhesion are solved, and the flexibility and energy density are improved. Enhanced battery performance.

CN119072800APending Publication Date: 2024-12-03LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380038466.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-02
Filing Date
2023-12-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The positive electrode of lithium secondary battery is prone to cracks and insufficient adhesion during the manufacturing process, resulting in low flexibility and difficulty in improving energy density.

Method used

Using a layer of positive electrode active material containing lithium transition metal phosphate and fluorine-containing adhesive, the flexibility and adhesion of the positive electrode are improved by adjusting the porosity and adhesive molecular weight, ensuring that the P/D value is within the range of 12.5 to 36, and increasing the The loading of lithium transition metal phosphate is provided, and conductive material and dispersant are added to the material layer to improve adhesion.

Benefits of technology

It effectively reduces the risk of cracks in the positive electrode during bending, improves energy density and adhesion, enhances the capacity and output characteristics of the battery, and reduces defects in the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

A positive electrode according to one embodiment of the present invention is a positive electrode comprising a positive electrode active material layer provided on at least one surface of a positive electrode current collector, the positive electrode active material layer comprising a lithium transition metal phosphate and a fluorine-containing binder, and in a flexible evaluation in which the positive electrode is lifted after the measurement rod of each phi (phi) is brought into contact with the positive electrode active material layer, the ratio (= P / D) of the porosity (P) of the positive electrode active material layer calculated by the disclosed formula 1 to the maximum phi value (D) of the measurement rod in which the crack occurs (= P / D) is greater than or equal to 10. [Formula 1] Porosity (P) = {1-(measured density of the positive electrode active material layer / true density of the positive electrode active material)} 100.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims priority to Korean Patent Application No. 10-2022-0166703, filed on December 2, 2022, the disclosure of which is incorporated herein by reference.

[0002] The present invention relates to a positive electrode and a lithium secondary battery manufactured using the same, and more particularly to a positive electrode having excellent flexibility and positive electrode adhesion, thereby reducing the risk of cracks in the positive electrode during the manufacturing process, and a lithium secondary battery with increased energy density. Background Art

[0003] With the technological development and increase in demand for electric vehicles and energy storage systems (ESS), the demand for batteries as energy sources has increased rapidly, and accordingly, various studies on batteries that can meet different needs are also being conducted. In particular, lithium secondary batteries with high energy density and excellent life and cycle characteristics as power sources for these devices are actively studied.

[0004] As a positive electrode active material of a lithium secondary battery, lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (LNCMO), lithium transition metal phosphate, etc. have been used.

[0005] Lithium transition metal phosphate is inexpensive because it is abundant in resources and contains a cheap material. In addition, since lithium transition metal phosphate has low toxicity, environmental pollution can be reduced when using lithium transition metal phosphate. In addition, since lithium transition metal phosphate has an olivine structure, the active material structure can remain stable at high temperatures compared to lithium transition metal oxides having a layered structure. Accordingly, lithium transition metal phosphate has an advantage in that the battery exhibits excellent high temperature stability and high temperature life characteristics.

[0006] However, since lithium transition metal phosphates have poor lithium mobility and low electrical conductivity compared to lithium transition metal oxides such as lithium cobalt oxide (LCO) and lithium nickel cobalt manganese oxide (LNCMO), lithium transition metal phosphates with a small average particle size are mainly used as positive electrode active materials. However, when the scale of lithium transition metal phosphate particles is reduced, the specific surface area increases, and accordingly, particle agglomeration occurs seriously. As a result, lithium transition metal phosphates and binders are not effectively mixed, and therefore, positive electrode adhesion is reduced. Therefore, the positive electrode active material layer will be separated when the electrode is manufactured or during the charge and discharge process, thereby increasing the battery resistance and reducing the capacity of the secondary battery.

[0007] In addition, compared with a positive electrode containing lithium cobalt oxide (LCO) or lithium nickel cobalt manganese oxide (LNCMO) as a positive electrode active material, a positive electrode containing lithium transition metal phosphate as a positive electrode active material has a low calendering density, and when the calendering density increases, the flexibility decreases, and therefore, during the calendering and slitting process, it is difficult to increase the calendering density due to the detachment of the positive electrode active material layer. Accordingly, it is difficult to increase the energy density of the battery, especially when manufactured as a wound electrode assembly, there is a high risk of rupture in the positive electrode due to the low flexibility.

[0008] In order to improve the flexibility of lithium transition metal phosphate positive electrodes, a technology of selecting a high molecular weight polymer binder has been studied, but the high molecular weight binder causes the viscosity of the positive electrode slurry to increase rapidly after mixing the slurry, resulting in a decrease in the coating productivity of the slurry. However, when the solid content in the slurry is reduced to reduce the viscosity of the positive electrode slurry, there is a problem that drying takes time due to the increase in solvent.

[0009] Therefore, it is necessary to develop a technology for improving the flexibility and adhesion of the positive electrode without causing a decrease in the coating and drying productivity of the positive electrode. Summary of the invention

[0010] Technical issues

[0011] The present invention aims to provide a positive electrode having improved flexibility and adhesion without causing a decrease in coating and drying productivity of the positive electrode, and a lithium secondary battery having improved energy density.

[0012] Technical Solution

[0013] The present invention provides a positive electrode, the positive electrode comprising a positive electrode active material layer disposed on at least one surface of a positive electrode current collector. The positive electrode active material layer comprises a lithium transition metal phosphate and a fluorine-containing binder, and in a flexibility evaluation of the positive electrode lifted after a measuring rod of each phi (Φ) is brought into contact with the positive electrode active material layer, the ratio (=P / D) of the porosity (P) of the positive electrode active material layer calculated by the following formula 1 to the maximum phi value (D) of the measuring rod where cracks occur is greater than or equal to 10.

[0014] [Formula 1]

[0015] Porosity (P) = {1-(measured density of the positive electrode active material layer / true density of the positive electrode active material)}×100.

[0016] In the positive electrode according to some embodiments, the P / D value may be in the range of 12.5 to 36.

[0017] In the positive electrode according to some embodiments, the porosity (P) of the positive electrode active material layer calculated by Formula 1 may be greater than or equal to 27%.

[0018] In the positive electrode according to some embodiments, the porosity (P) of the positive electrode active material layer calculated by Formula 1 may be in the range of 28% to 36%.

[0019] In the positive electrode according to some embodiments, the fluorine-containing binder may include a first fluorine-containing binder having a weight average molecular weight (Mw) of 500,000 to 750,000 g / mol and a second fluorine-containing binder having a weight average molecular weight (Mw) of 800,000 g / mol or more.

[0020] In the positive electrode according to some embodiments, the weight average molecular weight (Mw) of the second fluorine-containing binder may be 850,000 g / mol to 2,000,000 g / mol.

[0021] In the positive electrode according to some embodiments, a ratio (=B / A) of the weight of the lithium transition metal phosphate (B) to the total weight of the fluorine-containing binder (A) may be in the range of 27 to 98.

[0022] In the positive electrode according to some embodiments, a ratio (=B / A) of the weight of the lithium transition metal phosphate (B) to the total weight of the fluorine-containing binder (A) may be in the range of 30 to 65.

[0023] In the positive electrode according to one embodiment, in the flexibility evaluation in which the positive electrode is lifted after the measuring rods of each phi (Φ) are brought into contact with the positive electrode active material layer, cracks may occur in the measuring rods of 3 phi (Φ) or less.

[0024] In the positive electrode according to some embodiments, the lithium transition metal phosphate may be represented by the following Chemical Formula 1,

[0025] [Chemical formula 1]

[0026] Li 1+a M1 1-x M2 x (PO y-b )D b

[0027] Wherein, in Chemical Formula 1,

[0028] M1 may be at least one element selected from Fe, Mn, Co, Ni, Cu, Zn and Mg,

[0029] M2 may be selected from Group 2 to Group 15, and may be one or more elements other than element M1,

[0030] D may be at least one element selected from F, S and N, and

[0031] a, x, y and b may satisfy -0.5≤a≤0.5, 0≤x≤0.8, 3.95≤y≤4.05 and 0≤b≤1 respectively.

[0032] In the positive electrode according to some embodiments, the loading amount of the positive electrode active material layer may be 400 mg / 25 cm 2 Up to 700 mg / 25 cm 2 within the range.

[0033] In the positive electrode according to some embodiments, the positive electrode active material layer may further include a conductive material, and the conductive material may be a carbon nanotube.

[0034] In the positive electrode according to some embodiments, the content of the conductive material in the positive electrode active material layer may be 0.5 wt % to 1.3 wt %.

[0035] In the positive electrode according to some embodiments, the positive electrode active material layer may further include hydrogenated nitrile butadiene rubber.

[0036] According to some aspects of the present invention, a lithium secondary battery including the positive electrode is provided.

[0037] Beneficial Effects

[0038] The positive electrode according to the present invention has improved flexibility, and thus the risk of breakage during bending can be reduced.

[0039] Furthermore, the positive electrode according to the present invention has improved adhesion, and thus the weight ratio of the lithium transition metal phosphate contained in the positive electrode active material layer can be increased without decreasing the adhesion, thereby improving energy density. DETAILED DESCRIPTION

[0040] The advantages and features of the present invention and methods for achieving them will be apparent from the exemplary embodiments described in detail below. However, the present invention is not limited to the exemplary embodiments described below and may be implemented in various forms. On the contrary, embodiments are provided to make the disclosure of the present invention detailed and complete and to fully inform the scope of the present invention to those of ordinary skill in the art to which the present invention belongs, and the present invention is limited only by the scope of the claims.

[0041] Unless otherwise defined, all terms (including technical or scientific terms) used herein should be interpreted as having the same meaning as those generally understood by those skilled in the art to which the present invention belongs. In addition, unless clearly defined, terms such as terms defined in commonly used dictionaries cannot be ideally or over-interpreted.

[0042] The terms used herein are used to describe embodiments and are not intended to limit the present invention. In this specification, unless otherwise specified in a phrase, a singular form may include a plural form. As used herein, the terms "comprise" and / or "include" do not exclude the presence or addition of one or more other components other than the described components.

[0043] In the present specification, when an ingredient is referred to as “containing,” “including,” “comprising,” or “having” another ingredient, it should be understood that the ingredient does not exclude other ingredients but may include other ingredients unless explicitly stated otherwise.

[0044] In this specification, reference to "A and / or B" means A, B, or A and B.

[0045] In the present specification, "%" means weight % unless otherwise specifically stated.

[0046] In this manual, D 50 It refers to the particle size corresponding to 50% cumulative volume in the particle size distribution curve. For example, D can be measured by laser diffraction. 50 Laser diffraction is generally capable of measuring particle sizes ranging from submicrometers to several millimeters, and can produce results with high reproducibility and high resolution.

[0047] In this specification, "phi (Φ)" refers to the diameter of a particular measuring rod in millimeters (mm).

[0048] In this specification, the "specific surface area" is measured by the Brunauer-Emmett-Teller (BET) method, specifically, can be calculated from the amount of nitrogen adsorbed at liquid nitrogen temperature (77 K) using BELSORP-mini II available from BEL Japan.

[0049] In this specification, "weight average molecular weight (Mw)" refers to a conversion value relative to standard polystyrene measured by gel permeation chromatography (GPC). Specifically, the weight average molecular weight is a value obtained by converting the value measured using GPC under the following conditions, and a calibration curve is prepared using standard polystyrene of an Agilent system.

[0050] <Measurement conditions>

[0051] Measuring instrument: Agilent GPC (Agilent 1200 series, USA)

[0052] Column: Two connected PL mixed B

[0053] Column temperature: 40°C

[0054] Eluent: Tetrahydrofuran

[0055] Flow rate: 1.0 mL / min

[0056] Concentration: ~1 mg / mL (100 μL injection)

[0057] In this specification, the positive electrode flexibility can be measured as follows. A measuring rod of each phi (Φ) is prepared and a loading amount of 600 mg / 25 cm 2 The positive electrode is cut into a width of 10 cm and a length of 30 cm. The cut positive electrode is bent in half and the measuring rod is brought into contact with it, and then both ends of the positive electrode are lifted at a speed of 10 mm / min. At this time, both ends of the positive electrode are lifted until the force measured by the universal testing machine (UTM) reaches 5 N. Whether cracks appear in each phi electrode is observed by an optical microscope, and when there are no cracks, a measuring rod with a smaller phi is used for measurement. In addition, the diameters of the measuring rods are 1Φ, 1.5Φ, 2Φ, 2.5Φ, 3Φ, 4Φ, 5Φ, 6Φ and 7Φ, respectively.

[0058] In this specification, the porosity of the positive electrode active material layer can be defined by the following formula 1, in which the "measured density of the positive electrode active material layer" is a value calculated by measuring the weight and volume of the positive electrode active material layer separated from the positive electrode collector of the positive electrode after calendering, and the "true density of the positive electrode active material" is the density relative to the volume of the positive electrode active material particles themselves (excluding pores), and can be measured using a densitometer (AccuPycII 1340).

[0059] Porosity (P) = {1-(measured density of the positive electrode active material layer / true density of the positive electrode active material)}×100.

[0060] Hereinafter, the present invention will be described in more detail.

[0061] positive electrode

[0062] According to some embodiments of the present invention, the positive electrode is a positive electrode comprising a positive electrode active material layer arranged on at least one surface of a positive electrode collector, wherein the positive electrode active material layer comprises a lithium transition metal phosphate and a fluorine-containing binder, and in an evaluation of the flexibility of the positive electrode when a measuring rod of each phi (Φ) is brought into contact with the positive electrode active material layer and then lifted up, the ratio (=P / D) of the porosity P of the positive electrode active material layer calculated by the following formula 1 to the maximum phi value D of the measuring rod where cracks occur can be greater than or equal to 10.

[0063] [Formula 1]

[0064] Porosity (P) = {1-(measured density of the positive electrode active material layer / true density of the positive electrode active material)}×100.

[0065] Since the flexibility evaluation method has been described above, a repeated description will be omitted here.

[0066] Since the lithium transition metal phosphate used as the positive electrode active material is a fine particle compared to lithium nickel cobalt manganese oxide, the viscosity of the positive electrode slurry containing the lithium transition metal phosphate is significantly higher than that of the positive electrode slurry containing lithium nickel cobalt manganese oxide. Therefore, in general, when preparing the positive electrode slurry containing the lithium transition metal phosphate as the positive electrode active material, a fluorine-containing binder having a weight average molecular weight (Mw) of 750,000 g / mol or less is generally selected as the binder in consideration of manufacturing processability.

[0067] On the other hand, compared with a positive electrode containing lithium cobalt oxide (LCO) or lithium nickel cobalt manganese oxide (LNCMO) as a positive electrode active material, a positive electrode containing lithium transition metal phosphate as a positive electrode active material has a low rolling density, and when the rolling density increases, the flexibility decreases, and therefore, there is a risk of cracks occurring in the positive electrode when made into a jelly-roll type.

[0068] The inventors of the present invention have found that controlling the P / D value to an appropriate value, such as greater than 10, leads to improved flexibility and adhesion of the positive electrode. In some exemplary embodiments, the P / D value can be adjusted to a range of 12.5 to 36. As the P / D value increases, better flexibility of the positive electrode is obtained, but when the P / D value is too large, the energy density of the positive electrode is too low, which is not preferred. On the contrary, when the P / D value decreases and the positive electrode is subjected to a physical external force such as bending deformation, the capacity and adhesion strength may decrease due to cracks in the positive electrode. Therefore, controlling the P / D value balances the energy characteristics with the physical durability, and allows the production of a positive electrode having both favorable energy density and flexibility.

[0069] The positive electrode according to some embodiments of the present invention may include a positive electrode active material layer. Specifically, the positive electrode according to the present invention may include a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector.

[0070] There is no particular limitation on the positive electrode current collector as long as it does not cause chemical changes in the battery and has conductivity. For example, the following can be used as the positive electrode current collector: stainless steel, aluminum, nickel, titanium, sintered carbon; or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc.

[0071] The thickness of the positive electrode current collector may be 3 μm to 500 μm, and fine concavoconvexities may be formed on its surface to increase the adhesion with the positive electrode active material layer. For example, the positive electrode current collector may be used in various forms, such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0072] In the positive electrode according to the present invention, in order to improve flexibility, the porosity P of the positive electrode active material layer calculated by the above formula 1 may be 27% or more, preferably 28% to 36%. When the porosity P of the positive electrode active material layer is less than 27%, the flexibility of the positive electrode is reduced, and therefore, cracks may occur in the positive electrode during the manufacturing process of the jelly roll type electrode assembly, and when the porosity P of the positive electrode active material layer is greater than 36%, the energy density of the positive electrode may be reduced, which is not preferred.

[0073] In the manufacturing process of the positive electrode, by appropriately adjusting the thickness change rate of the positive electrode active material layer before and after calendering and the load of the positive electrode active material layer during the calendering process, the porosity of the positive electrode active material layer can be within the above numerical range. Specifically, the porosity of the positive electrode active material layer can decrease with the increase of the thickness change rate or load of the positive electrode active material layer before / after calendering, and the porosity of the positive electrode active material layer can increase with the decrease of the thickness change rate or load of the positive electrode active material layer before / after calendering.

[0074] In some embodiments, the loading of the positive electrode active material layer can be 400 mg / 25 cm 2 Up to 750 mg / 25cm 2 In the range of 450 mg / 25 cm 2 Up to 700 mg / 25 cm 2 The loading amount within the above range is greater than that of a conventional positive electrode, and thus is suitable as a high-load positive electrode.

[0075] The positive electrode according to the present invention can have flexibility when a flexibility test is performed in which the positive electrode is lifted up after a measuring rod of each phi is brought into contact with the positive electrode active material layer, wherein cracks are generated with a measuring rod of 3 phi (Φ) or less, but no cracks are generated with a measuring rod of more than 3 phi (Φ).

[0076] According to the present invention, the positive electrode has a P / D value greater than or equal to 10, and thus has both appropriate energy density and excellent flexibility, thereby reducing the crack rate of the positive electrode during bending deformation, thereby preventing the positive electrode from detaching during the positive electrode manufacturing process.

[0077] The positive electrode according to the present invention has an adhesive strength between the positive electrode current collector and the positive electrode active material layer as measured by a 90° peel test of 17 gf / 20 mm or more, specifically 20 gf / 20 mm or more, more specifically 20 gf / 20 mm to 100 gf / 20 mm.

[0078] The positive electrode according to the present invention has excellent positive electrode adhesion and flexibility, and as a result, a high-load positive electrode can be manufactured and positive electrode detachment can be prevented, thereby reducing the battery resistance of the secondary battery, enhancing the capacity and output characteristics of the battery, and reducing defects generated during the manufacturing process.

[0079] Hereinafter, each component included in the positive electrode active material layer will be described in detail.

[0080] (1) Positive electrode active material

[0081] The present invention includes a lithium transition metal phosphate as a positive electrode active material. The lithium transition metal phosphate has an olivine structure, so the active material structure remains stable at high temperatures compared to a lithium transition metal oxide having a layered structure. As a result, when the lithium transition metal phosphate is used as a positive electrode active material, the high temperature stability and high temperature life characteristics of the positive electrode are significantly improved, thereby reducing the fire risk of a lithium secondary battery including the positive electrode.

[0082] The lithium transition metal phosphate may be a compound represented by Chemical Formula 1 below.

[0083] [Chemical formula 1]

[0084] Li 1+a M1 1-x M2 x (PO y-b )D b

[0085] Wherein, in Chemical Formula 1,

[0086] M1 may be at least one element selected from Fe, Mn, Co, Ni, Cu, Zn and Mg,

[0087] M2 may be selected from Group 2 to Group 15, and may be one or more elements other than element M1,

[0088] D may be at least one element selected from F, S and N, and

[0089] a, x, y and b may satisfy -0.5≤a≤0.5, 0≤x≤0.8, 3.95≤y≤4.05 and 0≤b≤1 respectively.

[0090] In the lithium transition metal phosphate according to some embodiments of the present invention, M1 may be Fe, and M2 may be one or more selected from Al, Mg, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn, and Y. Specifically, the lithium transition metal phosphate may be lithium iron phosphate (LiFePO4).

[0091] The lithium transition metal phosphate may be a secondary particle in which primary particles are aggregated with each other, and preferably, may have a single body structure composed of primary particles.

[0092] In this specification, "monolith structure" means a structure of morphologically independent phases in which particles are not aggregated with each other. Particle structures in contrast to monolithic structures may include structures in which relatively large-sized particle shapes (secondary particles) are formed by physical and / or chemical aggregation of relatively small-sized particles (primary particles).

[0093] When the lithium transition metal phosphate has a single body structure consisting of primary particles, the lithium transition metal phosphate particles are less likely to break during the rolling process, and the capacity reduction caused by the detachment of the broken particles is small, which is preferred. In addition, when the lithium transition metal phosphate has primary particles of a single body structure, the binder migration during the drying process of the positive electrode slurry can be alleviated, which is preferred in terms of the interfacial adhesion between the positive electrode collector and the positive electrode active material layer.

[0094] The lithium transition metal phosphate may include a carbon coating on its surface. When the carbon coating is formed on the surface of the lithium transition metal phosphate, the electrical conductivity may be improved, thereby improving the resistance characteristics of the positive electrode.

[0095] The carbon coating layer can be formed using one or more raw materials selected from glucose, sucrose, lactose, starch, oligosaccharides, polyoligosaccharides, fructose, cellulose, furfuryl alcohol polymers, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, asphalt resins, and tar-based resins. Specifically, the carbon coating layer can be formed by mixing the raw materials with lithium transition metal phosphate and performing a heat treatment process.

[0096] Average particle size D of lithium transition metal phosphate 50 The average particle size D of the positive electrode active material may be 0.8 μm to 20.0 μm, specifically 0.9 μm to 10.0 μm, and more specifically 0.9 μm to 3.0 μm. 50 When the above range is met, the mobility of lithium in the lithium transition metal phosphate is improved, so that the charge and discharge characteristics of the battery can be improved.

[0097] The BET surface area of ​​lithium transition metal phosphates can be 5 m 2 / g to 20 m 2 / g, specifically 7 m 2 / g to 18m 2 / g, more specifically 9 m 2 / g to 16 m 2 / g. Compared with conventional lithium transition metal phosphates, the above range corresponds to a lower value. When the above range is satisfied, even in a positive electrode slurry composition having a relatively small dispersant content, agglomeration of the lithium transition metal phosphate can be effectively suppressed.

[0098] Based on the total solid content of the positive electrode slurry composition, the content of the lithium transition metal phosphate may be 93 wt % to 99 wt %, specifically 94 wt % to 98 wt %, and more specifically 95 wt % to 98 wt %. When the content of the lithium transition metal phosphate satisfies the above range, the battery capacity of the positive electrode can be improved by ensuring sufficient positive electrode energy density.

[0099] (2) Adhesive

[0100] The positive electrode according to the present invention may contain a fluorine-containing binder as a binder, and preferably may contain two types of fluorine-containing binders having different weight average molecular weights.

[0101] Specifically, the positive electrode may include a first fluorine-containing binder having a weight average molecular weight (Mw) of 500,000 g / mol to 750,000 g / mol and a second fluorine-containing binder having a weight average molecular weight (Mw) of 800,000 g / mol or more.

[0102] The first fluorine-containing adhesive and the second fluorine-containing adhesive may each independently contain a polyvinylidene fluoride (PVdF)-based polymer containing vinylidene fluoride (VdF) as a monomer. Specific examples of PVdF-based polymers may include PVdF homopolymers, poly(vinylidene fluoride-to-hexafluoropropylene) (PVdF-HFP), poly(vinylidene fluoride-to-chlorotrifluoroethylene) (PVdF-CTFE), poly(vinylidene fluoride-to-tetrafluoroethylene) (PVdF-TFE), poly(vinylidene fluoride-to-trifluoroethylene) (PVdF-TrFE), etc.

[0103] The weight average molecular weight (Mw) of the first fluorine-containing binder may be 500,000 g / mol to 750,000 g / mol, preferably 530,000 g / mol to 730,000 g / mol, and more preferably 550,000 g / mol to 650,000 g / mol. The first fluorine-containing binder may be used to provide stability to the positive electrode slurry, and to provide adhesion between the positive electrode active material and the conductive material and between the current collector and the positive electrode active material layer.

[0104] In an exemplary embodiment, the first fluorine-containing binder may be a polyvinylidene fluoride (PVdF) homopolymer. Since the homopolymer of PVdF contains a small amount of polar functional groups such as -COOH, the functional groups of the binder can reduce the number of hydrogen bonds between hydrogen on the carbon coating coated on the surface of the lithium transition metal phosphate particles, thereby preventing the gelation of the positive electrode slurry and improving the coating processability of the positive electrode slurry. In addition, the thickness and / or surface of the coated positive electrode active material layer is uniform, so the output performance and life characteristics of the lithium secondary battery manufactured using the positive electrode are excellent.

[0105] The weight average molecular weight (Mw) of the second fluorine-containing binder may be 800,000 g / mol or more, preferably 850,000 g / mol to 2,000,000 g / mol, and more preferably 900,000 g / mol to 1,500,000 g / mol. The second fluorine-containing binder may improve the flexibility and adhesion of the positive electrode.

[0106] The second fluorine-containing adhesive may be a homopolymer or copolymer of polyvinylidene fluoride (PVdF), and in some embodiments of the present invention, the second fluorine-containing adhesive may be polyvinylidene fluoride (PVdF) containing a polar functional group. When the second fluorine-containing adhesive contains a polar functional group, the crystallinity of the second fluorine-containing adhesive is reduced, thereby improving the flexibility of the positive electrode active material layer. In addition, since the flexibility of the positive electrode active material layer is improved, the positive electrode active material layer will not be separated from the positive electrode current collector even when external stress is applied, and as a result, the adhesion of the positive electrode can be improved.

[0107] The polar functional group may be one or more selected from carboxylic acid groups, sulfonic acid groups, phosphonic acid groups, acid anhydride groups, hydroxyl groups and salts thereof, but is not necessarily limited thereto, and may be any polar functional group available in the art.

[0108] When a medium / low molecular weight first fluorine-containing binder having a weight average molecular weight (Mw) in the range of 500,000 g / mol to 750,000 g / mol and a high molecular weight second fluorine-containing binder having a weight average molecular weight (Mw) of 800,000 g / mol or more are used together, the flexibility of the positive electrode can be improved relative to the prior art in which only a medium / low molecular weight fluorine-containing binder is selected as a binder. In an exemplary embodiment, the weight ratio of the first fluorine-containing binder to the second fluorine-containing binder may be 65:35 to 1:4, preferably 1:1 to 1:4, and more preferably 1:1 to 1:3. When the weight ratio of the first fluorine-containing binder to the second fluorine-containing binder exceeds 65:35 and the content of the first fluorine-containing binder is too large, it is not preferred in terms of the flexibility of the positive electrode, and when the weight ratio of the first fluorine-containing binder to the second fluorine-containing binder is less than 1:4 and the content of the second fluorine-containing binder is too large, gelation of the positive electrode slurry may occur, so it is not preferred.

[0109] The first fluorine-containing binder and the second fluorine-containing binder may be contained in the positive electrode active material layer such that the total weight of the first fluorine-containing binder and the second fluorine-containing binder is in the range of 1.0 wt % to 4.0 wt %, preferably in the range of 1.2 wt % to 3.5 wt %, more preferably in the range of 1.4 wt % to 3.0 wt %.

[0110] In addition, the ratio of the weight B of the lithium transition metal phosphate as the positive electrode active material to the total weight A of the first fluorine-containing binder and the second fluorine-containing binder may be in the range of 27 to 98, preferably in the range of 30 to 65, and more preferably in the range of 32 to 48.5. Since the positive electrode of the present invention includes the fluorine-containing binders having different weight average molecular weight ranges, the adhesion of the positive electrode can be improved, thereby increasing the weight ratio of the positive electrode active material contained in the positive electrode active material layer, thereby increasing the unit weight energy density of the positive electrode.

[0111] (3) Conductive materials

[0112] The positive electrode active material layer of the present invention may further contain a conductive material.

[0113] There is no particular limitation on the conductive material as long as it imparts conductivity without causing chemical changes in the battery, and may be, for example: graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fibers such as carbon fibers or metal fibers; fluorocarbons; metal powders such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. Specific examples of commercially available conductive materials may include acetylene black-based products (available from Chevron Chemical, Denka Singapore Pte Ltd. (Denka Black) and Gulf Oil), Ketjen black, EC series (available from Armak), Vulcan XC-72 (available from Cabot), Super P (available from Timcal Ltd.), etc. Preferably, the conductive material may be a carbon nanotube. When the conductive material is carbon nanotubes, the excellent conductive network of carbon nanotubes can suppress the binder migration phenomenon (in which the binder moves toward the electrode surface when the electrode is dried), thereby further improving the interfacial adhesion between the positive current collector and the positive active material layer.

[0114] The content of the conductive material in the positive electrode active material layer may be 0.3 wt % to 2.0 wt %, specifically 0.4 wt % to 1.5 wt %, more specifically 0.5 wt % to 1.3 wt %. When the content of the conductive material in the positive electrode active material layer satisfies the above range, the conductive network of the positive electrode is ensured, so the conductivity of the positive electrode can be improved.

[0115] According to some embodiments of the present invention, the positive electrode active material layer may include 94.9% to 97.2% by weight of the positive electrode active material, 0.8% to 1.3% by weight of the conductive material and 2.0% to 3.5% by weight of the binder. When the composition in the positive electrode active material layer meets the above range, the adhesion and conductivity of the electrode are ensured, while the active material content is increased, thereby balancing the capacity and resistance performance of the lithium secondary battery comprising the positive electrode.

[0116] (4) Dispersant

[0117] The positive electrode active material layer of the present invention may further contain a dispersant.

[0118] The dispersant suppresses a phenomenon in which the lithium transition metal phosphate is excessively agglomerated in the positive electrode slurry composition, allowing the lithium transition metal phosphate to be effectively dispersed and present in the prepared positive electrode active material layer.

[0119] The dispersant may include a hydrogenated nitrile copolymer. Specifically, the dispersant may be a hydrogenated nitrile copolymer.

[0120] Specifically, the hydrogenated nitrile copolymer can be a copolymer comprising a structural unit derived from an α, β-unsaturated nitrile and a structural unit derived from a hydrogenated conjugated diene, or a copolymer comprising a structural unit derived from an α, β-unsaturated nitrile, a structural unit derived from a conjugated diene, and a structural unit derived from a hydrogenated conjugated diene. As an α, β-unsaturated nitrile monomer, for example, acrylonitrile, methacrylonitrile, etc. can be used, and they can be used alone or in a mixture of two or more thereof. As a conjugated diene monomer, for example, a C4 to C6 conjugated diene monomer such as 1,3-butadiene, isoprene, 2,3-methylbutadiene, etc. can be used, and they can be used alone or in a mixture of two or more thereof.

[0121] More specifically, the hydrogenated nitrile copolymer may be hydrogenated nitrile butadiene rubber (H-NBR).

[0122] Based on the total solid content of the positive electrode slurry composition, the content of the dispersant may be 0.1 wt % to 2.0 wt %, specifically 0.2 wt % to 1.8 wt %, more specifically 0.3 wt % to 1.6 wt %. When the content of the dispersant satisfies the above range, agglomeration of the positive electrode active material may be suppressed, thereby preventing the positive electrode slurry composition from gelling.

[0123] The positive electrode according to the present invention can be manufactured according to a conventional method for manufacturing a positive electrode. Specifically, by preparing a positive electrode slurry composition comprising a positive electrode active material, a conductive material, a binder and / or a dispersant, applying the positive electrode slurry composition to a positive electrode collector, and then drying and rolling, a positive electrode can be manufactured.

[0124] Furthermore, as another method, the positive electrode may be manufactured by casting the positive electrode slurry composition on a separate support and then laminating the film peeled off from the support on a positive electrode collector.

[0125] Lithium secondary battery

[0126] Next, a lithium secondary battery according to the present invention will be described.

[0127] A lithium secondary battery according to some embodiments of the present invention may include a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.

[0128] In a lithium secondary battery, the positive electrode is the same as described above. For example, the positive electrode comprises a positive electrode active material layer disposed on at least one surface of a positive electrode current collector, wherein the positive electrode active material layer comprises a lithium transition metal phosphate and a fluorine-containing binder, and in the flexibility evaluation of the positive electrode after the measuring rods of each phi (Φ) are brought into contact with the positive electrode active material layer, the ratio (=P / D) of the porosity P of the positive electrode active material layer calculated by the following formula 1 to the maximum phi value D of the measuring rod where cracks occur can be greater than or equal to 10.

[0129] [Formula 1]

[0130] Porosity (P) = {1-(measured density of the positive electrode active material layer / true density of the positive electrode active material)}×100.

[0131] In addition, the positive electrode may further include a conductive material and a dispersant.

[0132] For example, the negative electrode may be manufactured by preparing a negative electrode-forming composition including a negative electrode active material, a negative electrode binder, and a negative electrode conductive material on a negative electrode current collector and then applying the composition to the negative electrode current collector.

[0133] There is no particular restriction on the negative electrode active material, and any compound that can reversibly embed and deintercalate lithium can be used. Specific examples thereof include: carbonaceous materials, such as artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, high crystallinity carbon, etc.; (semi)metallic materials that can be alloyed with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, Al alloy, etc.; or composite materials containing (semi)metallic materials and carbonaceous materials. In addition, examples of low-crystallinity carbon include soft carbon and hard carbon, and examples of high-crystallinity carbon include natural graphite, condensed graphite, pyrolytic carbon, mesophase pitch carbon fiber, mesophase carbon microbeads, mesophase pitch and high-temperature sintered carbon, such as coke derived from petroleum or coal tar pitch, which can be used alone or as a mixture of two or more thereof. In addition, as a negative electrode active material, a lithium metal film can be used.

[0134] The negative electrode conductive material is used to impart conductivity to the electrode, and any conductive material that does not cause chemical changes in the battery and has conductivity can be used without particular limitation. Specific examples of negative electrode conductive materials include graphite, such as natural graphite, artificial graphite, etc.; carbon materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, carbon nanotubes, etc.; metal powders or fibers, such as copper, nickel, aluminum, silver, etc.; conductive whiskers, such as zinc oxide, potassium titanate, etc.; conductive metal oxides, such as titanium oxide, etc.; and conductive polymers, such as polyphenylene derivatives, etc., which can be used alone or in mixtures of two or more thereof. Relative to the total weight of the negative electrode active material layer, the content of the negative electrode conductive material can generally be 1% to 30% by weight, specifically 1% to 20% by weight, and more specifically 1% to 10% by weight.

[0135] The negative electrode binder is used to enhance the cohesive force between the negative electrode active material particles and the adhesion between the negative electrode active material and the negative electrode collector. Specific examples of negative electrode binders include polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene rubber (EPDM rubber), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber and various copolymers thereof, which can be used alone or in a mixture of two or more thereof. Relative to the gross weight of the negative electrode active material layer, the content of the negative electrode binder can be 1% to 30% by weight, specifically 1% to 20% by weight, and more specifically 1% to 10% by weight.

[0136] On the other hand, there is no particular limitation on the negative electrode current collector as long as it does not cause chemical changes in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, sintered carbon, or copper or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used as the negative electrode current collector.

[0137] In addition, the thickness of the negative electrode current collector can be 3 μm to 500 μm, and like the positive electrode current collector, fine concavoconvexities can be formed on the surface of the negative electrode current collector to increase the binding force of the negative electrode active material. For example, the negative electrode current collector can be used in a variety of forms, including films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc.

[0138] On the other hand, as a separator in a lithium secondary battery, any separator commonly used as a separator in a lithium secondary battery can be used without particular restriction, and in particular, a separator showing low resistance to electrolyte ion migration and having excellent electrolyte impregnation ability is preferred. Specifically, a porous polymer film can be used, for example, a porous polymer film formed by polyolefin polymers such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers and ethylene / methacrylate copolymers, or a laminated structure with more than two layers thereof. In addition, a typical porous nonwoven fabric can be used, for example, a nonwoven fabric formed by high melting point glass fiber or polyethylene terephthalate fiber. In addition, the separator can be a porous film having a pore size of 0.01 μm to 10 μm and a thickness of 5 μm to 300 μm.

[0139] On the other hand, in a lithium secondary battery, the electrolyte may contain an organic solvent and a lithium salt generally used in an electrolyte, but is not particularly limited.

[0140] As an organic solvent, any solvent that can serve as a medium through which ions participating in the electrochemical reaction of the battery can migrate can be used without special restrictions. Specifically, as an organic solvent, ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; ether solvents such as dibutyl ether, tetrahydrofuran, etc.; ketone solvents such as cyclohexanone, etc.; aromatic hydrocarbon solvents such as benzene, fluorobenzene, etc.; or carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), etc. can be used.

[0141] Among these, carbonate solvents are preferably used, and more preferably a mixture of cyclic carbonates such as ethylene carbonate or propylene carbonate and low-viscosity linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) which have high ionic conductivity and high dielectric constant and can increase the charge / discharge performance of the battery.

[0142] There is no particular restriction on the lithium salt, as long as it is a compound that can provide lithium ions used in lithium secondary batteries. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. can be used as lithium salts. The lithium salt is preferably contained in the electrolyte at a concentration of about 0.6 mol% to 2 mol%.

[0143] In order to enhance the life characteristics of the battery, inhibit the decline of the battery capacity, enhance the discharge capacity of the battery, etc., in addition to the above-mentioned electrolyte components, the electrolyte may also contain one or more additives, such as pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, (condensed) glycol dimethyl ether, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted Oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In this case, the content of the additive may be 0.1 wt % to 5 wt % relative to the total weight of the electrolyte.

[0144] The lithium secondary battery according to the present invention can be manufactured by inserting a separator between the positive electrode and the negative electrode to form an electrode assembly, placing the electrode assembly in a cylindrical battery case or a prismatic battery case and injecting an electrolyte. Alternatively, a lithium secondary battery can be manufactured by stacking electrode assemblies, impregnating them with an electrolyte, placing the resultant in a battery case and sealing the battery case.

[0145] When manufacturing a lithium secondary battery according to the present invention, the electrode assembly may be dried to remove one or more organic solvents selected from N-methyl-2-pyrrolidone (NMP), acetone, ethanol, propylene carbonate, ethyl methyl carbonate, ethylene carbonate and dimethyl carbonate used to manufacture the positive electrode. When an electrolyte having the same composition as the organic solvent used to manufacture the positive electrode is used as the electrolyte, the process of drying the electrode assembly may be omitted.

[0146] Unlike the above-described lithium secondary battery, a lithium secondary battery according to another embodiment of the present invention may be an all-solid-state battery.

[0147] As the battery case, any battery case commonly used in the art can be used, and there is no limitation on the external shape according to the purpose of the battery. For example, the external shape of the battery case can be a cylindrical shape using a can, a prismatic shape, a bag shape, a coin shape, etc.

[0148] The lithium secondary battery according to the present invention can be used in portable devices such as mobile phones, notebook computers, digital cameras, etc., energy storage systems (ESS), and electric vehicles such as hybrid electric vehicles (HEV) and the like because it stably exhibits excellent discharge capacity, output characteristics and excellent capacity retention rate.

[0149] The present invention will be described in more detail below with reference to Examples. However, the following Examples are provided only to illustrate the present invention, and the scope of the present invention is not limited to the following Examples.

[0150] Example 1: Preparation of positive electrode

[0151] (1) Preparation of positive electrode slurry

[0152] The average particle size D of the lithium transition metal phosphate 50 LiFePO4 of a primary particle of a single body structure of 1.0 μm, carbon nanotubes (CNT) as a conductive material, polyvinylidene fluoride (PVdF) having a weight average molecular weight (Mw) of 630,000 g / mol and being a homopolymer as a first fluorine-containing binder, and polyvinylidene fluoride (PVdF) having a weight average molecular weight (Mw) of 1,000,000 g / mol as a second fluorine-containing binder were added to an N-methylpyrrolidone (NMP) solvent. A homodispersor was used and mixed at 2500 rpm for 90 minutes to prepare a positive electrode slurry.

[0153] In the positive electrode slurry, the lithium transition metal phosphate, the conductive material, the first fluorine-containing binder, and the second fluorine-containing binder are present in a weight ratio of 96.6:1.0:1.25:1.25, and the solid content of the positive electrode slurry is 62 wt %.

[0154] (2) Manufacturing of positive electrode

[0155] The cathode slurry was coated onto a 20 μm thick aluminum film to achieve a density of 600 mg / 25 cm 2 , and then hot-air dried at 130°C for 5 minutes to make the solid content of the positive electrode slurry 99.0% by weight or more. Thereafter, the dried positive electrode slurry is rolled so that the porosity of the positive electrode active material layer is 29% to manufacture the positive electrode. Here, the porosity (P) is a value calculated by the following formula, the "measured density of the positive electrode active material layer" is a value calculated by measuring the weight and volume of the positive electrode active material layer separated from the positive electrode collector of the rolled positive electrode, and the "true density of the positive electrode active material" is the density relative to the volume of the positive electrode active material particles themselves (excluding pores), and can be measured using a densimeter (AccuPycII 1340).

[0156] Porosity (P) = {1-(measured density of the positive electrode active material layer / true density of the positive electrode active material)}×100.

[0157] Example 2: Preparation of positive electrode

[0158] A positive electrode was manufactured in the same manner as in Example 1, except that the porosity of the positive electrode active material layer was 32% when the dried positive electrode slurry was rolled.

[0159] Example 3: Preparation of positive electrode

[0160] A positive electrode was manufactured in the same manner as in Example 1, except that the second fluorine-containing binder was changed to polyvinylidene fluoride (PVDF) having a weight average molecular weight (Mw) of 880,000 when preparing the positive electrode slurry.

[0161] Example 4: Preparation of positive electrode

[0162] A positive electrode was manufactured in the same manner as in Example 1, except that, in preparing the positive electrode slurry, the first fluorine-containing binder was changed to polyvinylidene fluoride (PVDF) having a weight average molecular weight (Mw) of 700,000 and being a homopolymer.

[0163] Comparative Example 1: Preparation of positive electrode

[0164] (1) Preparation of positive electrode slurry

[0165] The average particle size D of the lithium transition metal phosphate 50 LiFePO4 of a single-body primary particle of 1.0 μm, carbon nanotubes (CNT) as a conductive material, and polyvinylidene fluoride (PVdF) with a weight average molecular weight (Mw) of 630,000 g / mol and a homopolymer as a fluorine-containing binder were added to an N-methylpyrrolidone (NMP) solvent. A homodispersor was used to mix at 2500 rpm for 90 minutes to prepare a positive electrode slurry.

[0166] In the positive electrode slurry, the lithium transition metal phosphate, the conductive material, and the fluorine-containing binder were present in a weight ratio of 96.5:1.0:2.5, and the solid content of the positive electrode slurry was 62 wt %.

[0167] (2) Manufacturing of positive electrode

[0168] The cathode slurry was coated onto a 20 μm thick aluminum film to achieve a density of 600 mg / 25 cm 2 The dried positive electrode slurry was then hot-dried at 130° C. for 5 minutes to make the solid content of the positive electrode slurry 99.0% by weight or more. The dried positive electrode slurry was then rolled to make the porosity of the positive electrode active material layer 29% to produce a positive electrode.

[0169] Comparative Example 2: Preparation of positive electrode

[0170] A positive electrode was manufactured in the same manner as in Example 1, except that the porosity of the positive electrode active material layer was 26% when the dried positive electrode slurry was rolled.

[0171] Experimental Example 1: Evaluation of the Flexibility of the Positive Electrode

[0172] Each of the positive electrodes manufactured in Examples 1 to 4 and Comparative Examples 1 and 2 was vacuum dried at a temperature of 130° C. for 2 hours, and the flexibility was measured. The results are shown in Table 1.

[0173] Specifically, measuring rods with diameters of 1Φ, 1.5Φ, 2Φ, 2.5Φ, 3Φ, 4Φ, 5Φ, 6Φ and 7Φ were prepared, and each positive electrode manufactured in Examples 1 to 4 and Comparative Examples 1 and 2 was cut into a width of 10 cm and a length of 30 cm. The cut positive electrode was bent in half and the measuring rod was brought into contact with it, and then both ends of the positive electrode were lifted at a speed of 10 mm / min. At this time, both ends of the positive electrode were lifted until the force measured by UTM reached 5 N. Whether cracks appeared in the electrodes of each phi was observed by an optical microscope, and when there were no cracks, a measuring rod with a smaller phi (Φ) was used for measurement. The maximum phi (Φ) value of the measuring rod that produced the crack is shown in Table 1.

[0174] In addition, the ratio (P / D) of the porosity P of the positive electrode active material layer to the maximum phi value D of the measuring rod where cracks occurred was calculated. The results are shown in Table 1.

[0175] Experimental Example 2: Adhesion Test of Positive Electrode

[0176] Each of the positive electrodes manufactured in Examples 1 to 4 and Comparative Examples 1 and 2 was vacuum dried at 130° C. for 2 hours, and then the adhesion between the positive electrode active material layer and the positive electrode current collector was measured. The results are shown in Table 1.

[0177] Specifically, each positive electrode manufactured in Examples 1 to 4 and Comparative Examples 1 and 2 was cut into a length of 150 mm and a width of 20 mm, and the positive electrode surface was pasted on a slide glass of 75 mm in length and 25 mm in width in the length direction using double-sided tape. That is, the slide glass was pasted to an area corresponding to half of the length direction of the positive electrode. In addition, a roller was used to perform 10 frictions so that the double-sided tape was evenly pasted to prepare an evaluation sample.

[0178] Next, the slide glass portion of the evaluation sample was fixed to the sample stage of the universal testing machine (UTM) (product name: LS5, manufacturer: LLOYD), and the half of the positive electrode that was not attached to the slide glass was connected to the load cell of the UTM. While moving the load cell upward by 50 mm at a 90 ° angle and a speed of 100 mm / min, the load applied to the load cell was measured. In this case, the load average value measured in the 20 mm to 40 mm interval of the driving interval was obtained. The process was repeated a total of 5 times, and the average value was evaluated as the positive electrode adhesion (gf / 20 mm) of each sample.

[0179]

[0180] Referring to Table 1, although the positive electrodes according to Examples 1, 3 and 4 and the positive electrode according to Comparative Example 1 all have the same binder content and porosity values, since the positive electrode according to the embodiment satisfies the condition that the P / D value is greater than or equal to 10, the positive electrode according to the embodiment is evaluated as having superior adhesion and flexibility.

[0181] The positive electrode according to Comparative Example 2 had the most excellent adhesive strength because the porosity of the positive electrode was less than 26, but was evaluated to have the worst flexibility.

[0182] On the other hand, the positive electrode according to Example 2 was inferior in adhesive strength due to a decrease in the calendering density compared with the positive electrodes according to Example 1, Example 3, and Example 4, but was evaluated to have the best flexibility.

[0183] As described above, it was evaluated that the positive electrode according to the present invention can minimize the risk of cracking during the battery manufacturing process as a result of improved flexibility.

Claims

1. A positive electrode, comprising: a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, in, The positive electrode active material layer comprises a lithium transition metal phosphate and a fluorine-containing binder, and In the flexibility evaluation of the positive electrode in which the measuring rods of each phi (Φ) are brought into contact with the positive electrode active material layer and then the positive electrode is lifted up, the ratio (=P / D) of the porosity (P) of the positive electrode active material layer calculated by the following formula 1 to the maximum phi value (D) of the measuring rod where cracks occur is greater than or equal to 10, [Formula 1] Porosity (P) = {1-(measured density of the positive electrode active material layer / true density of the positive electrode active material)}×100.

2. The positive electrode according to claim 1, wherein The P / D value is in the range of 12.5 to 36.

3. The positive electrode according to claim 1, wherein The positive electrode active material layer has a porosity (P) calculated by Formula 1 of greater than or equal to 27%.

4. The positive electrode according to claim 1, wherein The positive electrode active material layer has a porosity (P) calculated by Formula 1 in the range of 28% to 36%.

5. The positive electrode according to claim 1, wherein The ratio of the weight (B) of the lithium transition metal phosphate to the total weight (A) of the fluorine-containing binder (=B / A) is in the range of 27 to 98.

6. The positive electrode according to claim 1, wherein The ratio (B / A) of the weight of the lithium transition metal phosphate to the total weight of the fluorine-containing binder is in the range of 30 to 65.

7. The positive electrode according to claim 1, wherein In the flexibility evaluation in which the positive electrode was lifted after a measuring rod of each phi (Φ) was brought into contact with the positive electrode active material layer, the maximum phi (Φ) value of the measuring rod in which cracks occurred was 3 phi (Φ) or less.

8. The positive electrode according to claim 1, wherein The lithium transition metal phosphate is represented by the following chemical formula 1: [Chemical formula 1] <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> 1+a <h2 style=";text-align:left;direction:ltr"> M1<h2 style=";text-align:left;direction:ltr"> 1-x <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> (PO<h2 style=";text-align:left;direction:ltr"> y-b <h2 style=";text-align:left;direction:ltr"> D)<h2 style=";text-align:left;direction:ltr"> b in, In Chemical Formula 1, M1 is at least one element selected from Fe, Mn, Co, Ni, Cu, Zn and Mg, M2 is selected from Group 2 to Group 15 and is one or more elements other than the element M1, D is at least one element selected from F, S and N, and a, x, y and b satisfy -0.5≤a≤0.5, 0≤x≤0.8, 3.95≤y≤4.05 and 0≤b≤1 respectively.

9. The positive electrode according to claim 1, wherein The loading amount of the positive electrode active material layer is 400 mg / 25 cm 2 Up to 700 mg / 25 cm 2 within the range.

10. The positive electrode according to claim 1, wherein The positive electrode active material layer further includes a conductive material, and the conductive material is a carbon nanotube.

11. The positive electrode according to claim 10, wherein The content of the conductive material in the positive electrode active material layer is 0.5 wt % to 1.3 wt %.

12. The positive electrode according to claim 1, wherein The positive electrode active material layer further includes hydrogenated nitrile butadiene rubber. 13 . A lithium secondary battery, comprising the positive electrode according to claim 1 ; and a negative electrode.