Porphyrin and zero-valent iron co-loaded tungsten trioxide composite material, preparation method thereof and application of porphyrin and zero-valent iron co-loaded tungsten trioxide composite material in phosphorus removal of water body
Through the use of porphyrin and zero-valent iron-collected tungsten trioxide composite materials, the problem of low phosphate removal efficiency in water bodies is solved, and an efficient and environmentally friendly phosphate removal effect is achieved, which is suitable for the application of water treatment systems.
Patent Information
- Application Number
- CN202411373193.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-29
AI Technical Summary
The prior art has low activity and limited adsorption capacity for using tungsten trioxide alone in water bodies, making it difficult to effectively remove phosphate, resulting in the intensification of the eutrophication problem of water bodies.
The tungsten trioxide composite material is used to co-load porphyrin and zero-valent iron to form a stable composite structure through physical adsorption and chemical adsorption. The electron transfer performance of porphyrin and the redox capacity of Fe0 are used to improve the selective adsorption of phosphate. ability.
It significantly improves the removal efficiency of phosphate, achieves efficient removal of phosphate, and the materials are economical and environmentally friendly, suitable for large-scale applications and integration of water treatment systems.
Smart Images

Figure CN119075922A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sewage treatment, and in particular to a porphyrin and zero-valent iron co-loaded tungsten trioxide composite material, a preparation method thereof, and an application thereof in water phosphorus removal. Background Art
[0002] With the development of agriculture and industry and the discharge of domestic sewage, the phosphorus concentration in water bodies has gradually increased, leading to the aggravation of the eutrophication problem of water bodies. The algal blooms and algae outbreaks caused by eutrophication of water bodies not only destroy the aquatic ecosystem, but also seriously affect the utilization of water resources and even threaten human health. Therefore, controlling phosphorus pollution in water bodies has become one of the research focuses in the field of environmental protection.
[0003] At present, the methods for removing phosphorus from water bodies mainly include chemical precipitation, biological dephosphorization and adsorption. Among them, the adsorption method has become a hot topic of research due to its simple operation, low cost and environmental friendliness. 3 ) As a transition metal oxide, it has broad application prospects in the field of environmental remediation due to its unique electronic structure and excellent catalytic performance. However, the use of tungsten trioxide alone in water treatment shows certain limitations, such as low activity and limited adsorption capacity. To overcome these shortcomings, researchers have tried to compound tungsten trioxide with other functional materials to improve its performance, but so far, no composite method that can effectively improve the adsorption capacity has been studied. Summary of the invention
[0004] The main purpose of the present invention is to provide a porphyrin and zero-valent iron co-loaded tungsten trioxide composite material with selective adsorption capacity for phosphate and higher phosphorus removal efficiency, as well as a preparation method and application thereof.
[0005] To achieve the above object, the present invention provides a method for preparing a composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide, comprising the following steps:
[0006] (1) Will WO 3 The powder was added to deionized water, then purged with nitrogen to remove dissolved oxygen, and then subjected to ultrasonic dispersion treatment to obtain WO 3 Dispersion A;
[0007] (2) dissolving porphyrin in an organic solvent to obtain a porphyrin solution B;
[0008] (3) Under stirring conditions, add porphyrin solution B to WO 3 Dispersion liquid A, then ultrasonic dispersion treatment, and then stirring treatment to obtain porphyrin-loaded WO 3 Solution C;
[0009] (4) Adding iron salt to porphyrin-loaded WO 3Solution C, and then stirred to obtain a mixed solution D;
[0010] (5) Adding a reducing agent to the mixed solution D, stirring the mixed solution, and then centrifuging the mixed solution. Washing, drying, and grinding the precipitate obtained by centrifugation to obtain the porphyrin and zero-valent iron co-loaded tungsten trioxide composite material.
[0011] Further, in step (1), the WO 3 The material-liquid ratio of powder to deionized water is 0.5-3 g: 100-500 mL.
[0012] Furthermore, in step (2), the organic solvent is any one of ethanol, dichloromethane, N,N-dimethylformamide, dimethyl sulfoxide or tetrahydrofuran, or a mixture of two or more thereof in any proportion; the porphyrin is any one of iron porphyrin, zinc porphyrin, cobalt porphyrin or nickel porphyrin, or a mixture of two or more thereof in any proportion, and the solid-liquid ratio of the porphyrin to the organic solvent is 0.05-2 g:50-500 mL.
[0013] Further, in step (3), the WO 3 The dosage ratio of dispersion A and porphyrin solution B is: 3 Powder Scale, Porphyrin and WO 3 The mass ratio of the powder is 0.1-0.2:1-1.5.
[0014] Furthermore, in step (4), the iron salt is FeSO 4 、FeCl 3 or Fe(NO 3 ) 3 Any one or a mixture of two or more in any proportion, wherein the iron salt and porphyrin loaded WO 3 The dosage ratio of solution C is: the iron element contained and WO 3 Powder meter, iron and WO 3 The mass ratio of the powder is 0.1-15g:0.5-30g.
[0015] Furthermore, in step (5), the reducing agent is any one of sodium borohydride, potassium borohydride, vitamin C, hydroxylamine hydrochloride, tea polyphenols, and ascorbic acid, or a mixture of two or more of them in any proportion, and the mass ratio of the reducing agent to the iron salt is 0.1-5g:0.1-10g.
[0016] The present invention also provides a porphyrin and zero-valent iron co-loaded tungsten trioxide composite material, which is prepared according to the above preparation method.
[0017] The present invention also provides the use of the above-mentioned porphyrin and zero-valent iron co-loaded tungsten trioxide composite material in phosphorus removal from water.
[0018] The present invention also provides a method for removing phosphate from water, comprising the following steps: adding the above-mentioned porphyrin and zero-valent iron co-loaded tungsten trioxide composite material into the phosphate-containing water body, and stirring the reaction at room temperature.
[0019] Furthermore, the phosphate concentration of the water body is controlled at 0.1-100 mg / L, the dosage of the composite material is 0.1-5.0 g / L, the reaction conditions are pH 5-10, stirring speed 50-300 r / min, and reaction time 30-120 min.
[0020] The composite material of the present invention is composed of porphyrin, zero-valent iron and WO 3 The porphyrin molecules are first loaded on WO by physical adsorption (such as van der Waals force, π-π interaction) and chemical adsorption (such as coordination bond). 3 The metal ions in the porphyrin molecules may interact with WO through coordination. 3 The oxygen atoms on the surface combine to form a stable composite structure. 0 The particles were deposited on porphyrin-loaded WO by reduction reaction. 3 superior.
[0021] Zero valent iron (Fe 0 ) has high redox capacity. In water environment, Fe 0 It is easy to react with dissolved oxygen or water molecules in water to produce ferrous ions (Fe 2+ ) and ferric ions (Fe 3+ ). The generated Fe 2+ and Fe 3+ Further with phosphate (PO 4 3- ) reacts to form an insoluble iron-phosphorus compound (FePO 4 ).Fe 2+ After oxidation, Fe 3+ It can also continue to react with phosphates to further enhance the phosphorus removal effect.
[0022] Porphyrin is a kind of macrocyclic conjugated compound with excellent electron transfer performance and certain adsorption capacity. Porphyrin can accelerate the Fe 0 Oxidized to Fe 2+ / Fe 3+The reaction of porphyrin can improve the precipitation efficiency of phosphate. In addition, the special macrocyclic structure of porphyrin enables the material to effectively identify and capture phosphate ions in water, avoiding the interference of other competitive ions, thereby enhancing the phosphorus removal effect. In addition, the rich π electron system in porphyrin can participate in the electron transfer process, enhance the overall reaction activity of the composite material, accelerate the decomposition of inorganic phosphorus, and thus achieve a more accurate phosphorus removal effect. The composite material of the present invention combines WO 3 adsorption, electron transfer properties of porphyrin and Fe 0 The reducing ability of the components and the synergistic effect of the components significantly improve the selective adsorption capacity of the material for phosphate, avoiding the interference of other competitive ions, thereby achieving a more precise phosphorus removal effect, and greatly improving the phosphorus removal efficiency, achieving efficient removal of phosphate. This advantage is particularly significant in the treatment of high-phosphorus polluted water.
[0023] The beneficial effects of the present invention are embodied in:
[0024] 1. By combining porphyrin, Fe 0 and WO 3 The composite material of the present invention exhibits a significant synergistic effect in phosphorus removal. Compared with a single material, the composite material of the present invention can achieve efficient phosphorus removal under various water quality conditions.
[0025] 2. Fe used in the present invention 0 and WO 3 All of them are cheap and readily available materials, and the preparation process is relatively simple, without the need for complex processes and expensive equipment. Therefore, the material has good economic efficiency in large-scale applications. In addition, the use of the material does not produce secondary pollution, meets environmental protection requirements, and is more environmentally friendly than some existing chemical treatment methods.
[0026] 3. The preparation process of the present invention is simple and easy to mass produce, and the design of the material takes into account the convenience of operation in the actual water treatment process. Therefore, the material has good industrial application potential and can be easily integrated into the existing water treatment system to quickly achieve technology promotion.
[0027] In summary, the present invention is superior to the prior art in terms of phosphorus removal efficiency, multifunctional treatment capacity, material selectivity, environmental protection and industrialization potential, and provides a scientific basis and practical method for the effective treatment of phosphorus pollution (such as sodium phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate) in water bodies (such as network sewage, rural sewage, tap water, river water, lake water, etc.). BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The Por-Fe prepared in Example 4 of the present invention 0 @WO 3 -4 transmission electron microscopy (TEM).
[0029] Figure 2 The Por-Fe prepared in Example 4 of the present invention 0 @WO 3 -4's X-ray diffraction pattern (XRD). DETAILED DESCRIPTION
[0030] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0031] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods; unless otherwise specified, the methods used in the examples of the present invention are methods known to those skilled in the art. Among them, the ultrasonic dispersion treatment uses an FS-450N ultrasonic material disperser.
[0032] Example 1
[0033] Preparation of porphyrin and zero-valent iron co-loaded tungsten trioxide composite material
[0034] The preparation method is as follows:
[0035] Step (1): Take 1g WO 3 The powder was dissolved in 200 mL of deionized water, purged with nitrogen for 30 min to remove dissolved oxygen, and ultrasonically dispersed for 1 h to ensure oxidation of WO 3 Fully dispersed in the solution to form a uniform WO 3 Dispersion A;
[0036] Step (2): dissolving 0.1 g of bis(tetrakis-p-chlorophenyl)ferroporphyrin in 50 mL of ethanol and stirring the mixture to form a porphyrin solution B;
[0037] Step (3): Under stirring, slowly add porphyrin solution B to WO 3 Dispersion A was ultrasonically dispersed for 30 min, and then stirred at 150 r / min for 3 h to form porphyrin-loaded WO 3 Solution C;
[0038] Step (4): Loading WO onto porphyrin 3 0.5 g of ferrous sulfate was added to solution C, followed by stirring at 200 r / min for 1 h to ensure that the iron salt was fully dissolved, to obtain a mixed solution D;
[0039] Step (5): 0.5 g of sodium borohydride was slowly added to the mixed solution D, and then stirred at a speed of 250 r / min for 2 h to deposit Fe 0 Porphyrin-loaded WO particles3 The surface was centrifuged, and the precipitate obtained by centrifugation was washed with deionized water, dried in a vacuum drying oven at 60°C, and then ground to obtain a composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide. Labeled as Por-Fe 0 @WO 3 -1, including porphyrin, Fe 0 with WO 3 The mass ratio is 0.1g:0.184g:1g.
[0040] Example 2
[0041] Preparation of porphyrin and zero-valent iron co-loaded tungsten trioxide composite material
[0042] The preparation method is as follows:
[0043] Step (1): Take 1.5 g WO 3 The powder was dissolved in 200 mL of deionized water, purged with nitrogen for 30 min to remove dissolved oxygen, and ultrasonically dispersed for 1 h to ensure oxidation of WO 3 Fully dispersed in the solution to form a uniform WO 3 Dispersion A;
[0044] Step (2): dissolving 0.1 g of bis(tetrakis-p-chlorophenyl)ferroporphyrin in 50 mL of ethanol and stirring the mixture to form a porphyrin solution B;
[0045] Step (3): Under stirring, slowly add porphyrin solution B to WO 3 Dispersion A was ultrasonically dispersed for 30 min, and then stirred at 150 r / min for 3 h to form porphyrin-loaded WO 3 Solution C;
[0046] Step (4): Loading WO onto porphyrin 3 0.5 g of ferrous sulfate was added to solution C, followed by stirring at 200 r / min for 1 h to ensure that the iron salt was fully dissolved, to obtain a mixed solution D;
[0047] Step (5): 0.5 g of sodium borohydride was slowly added to the mixed solution D, and then stirred at a speed of 250 r / min for 2 h to deposit Fe 0 Porphyrin-loaded WO particles 3 The surface was centrifuged, and the precipitate obtained by centrifugation was washed with deionized water, dried in a vacuum drying oven at 60°C, and then ground to obtain a composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide. Labeled as Por-Fe 0 @WO 3 -2, including porphyrin, Fe 0 with WO 3 The mass ratio is 0.1g:0.184g:1.5g.
[0048] Example 3
[0049] Preparation of porphyrin and zero-valent iron co-loaded tungsten trioxide composite material
[0050] The preparation method is as follows:
[0051] Step (1): Take 1g WO 3 The powder was dissolved in 200 mL of deionized water, purged with nitrogen for 30 min to remove dissolved oxygen, and ultrasonically dispersed for 1 h to ensure oxidation of WO 3 Fully dispersed in the solution to form a uniform WO 3 Dispersion A;
[0052] Step (2): dissolving 0.2 g of bis(tetrakis-p-chlorophenyl)ferroporphyrin in 100 mL of ethanol and stirring the mixture to form a porphyrin solution B;
[0053] Step (3): Under stirring, slowly add porphyrin solution B to WO 3 Dispersion A was ultrasonically dispersed for 30 min, and then stirred at 150 r / min for 3 h to form porphyrin-loaded WO 3 Solution C;
[0054] Step (4): Loading WO onto porphyrin 3 About 0.5 g of ferrous sulfate was added to solution C, and then stirred at a speed of 200 r / min for 1 h to ensure that the iron salt was fully dissolved, to obtain a mixed solution D;
[0055] Step (5): 0.5 g of sodium borohydride was slowly added to the mixed solution D, and then stirred at a speed of 250 r / min for 2 h to deposit Fe 0 Porphyrin-loaded WO particles 3 The surface was centrifuged, and the precipitate obtained by centrifugation was washed with deionized water, dried in a vacuum drying oven at 60°C, and then ground to obtain a composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide. Labeled as Por-Fe 0 @WO 3 -3, including porphyrin, Fe 0 with WO 3 The mass ratio is 0.2g:0.184g:1g.
[0056] Example 4
[0057] Preparation of porphyrin and zero-valent iron co-loaded tungsten trioxide composite material
[0058] The preparation method is as follows:
[0059] Step (1): Take 1.0 g WO 3The powder was dissolved in 200 mL of deionized water, purged with nitrogen for 30 min to remove dissolved oxygen, and ultrasonically dispersed for 1 h to ensure oxidation of WO 3 Fully dispersed in the solution to form a uniform WO 3 Dispersion A;
[0060] Step (2): dissolving 0.1 g of bis(tetrakis-p-chlorophenyl)ferroporphyrin in 50 mL of ethanol and stirring the mixture to form a porphyrin solution B;
[0061] Step (3): Under stirring, slowly add porphyrin solution B to WO 3 Dispersion A was ultrasonically dispersed for 30 min, and then stirred at 150 r / min for 3 h to form porphyrin-loaded WO 3 Solution C;
[0062] Step (4): Loading WO onto porphyrin 3 About 1.0 g of ferrous sulfate was added to solution C, and then stirred at a speed of 200 r / min for 1 h to ensure that the iron salt was fully dissolved, to obtain a mixed solution D;
[0063] Step (5): 1.0 g of sodium borohydride was slowly added to the mixed solution D, and then stirred at a speed of 250 r / min for 2 h to deposit Fe 0 Porphyrin-loaded WO particles 3 The surface was centrifuged, and the precipitate obtained by centrifugation was washed with deionized water, dried in a vacuum drying oven at 60°C, and then ground to obtain a composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide. Labeled as Por-Fe 0 @WO 3 -4, including porphyrin, Fe 0 with WO 3 The mass ratio is 0.1g:0.368g:1g.
[0064] Example 5
[0065] Preparation of porphyrin and zero-valent iron co-loaded tungsten trioxide composite material
[0066] The preparation method is as follows:
[0067] Step (1): Take 1g WO 3 The powder was dissolved in 200 mL of deionized water, purged with nitrogen for 30 min to remove dissolved oxygen, and ultrasonically dispersed for 1 h to ensure oxidation of WO 3 Fully dispersed in the solution to form a uniform WO 3 Dispersion A;
[0068] Step (2): dissolving 0.1 g of bis(tetrakis-p-chlorophenyl)iron porphyrin in 150 mL of ethanol and stirring the mixture to form a porphyrin solution B;
[0069] Step (3): Under stirring, slowly add porphyrin solution B to WO 3 Dispersion A was ultrasonically dispersed for 30 min, and then stirred at 150 r / min for 3 h to form porphyrin-loaded WO 3 Solution C;
[0070] Step (4): Loading WO onto porphyrin 3 About 1.5 g of ferrous sulfate was added to solution C, and then stirred at a speed of 200 r / min for 1 h to ensure that the iron salt was fully dissolved, to obtain a mixed solution D;
[0071] Step (5): 1.5 g of sodium borohydride was slowly added to the mixed solution D, and then stirred at a speed of 250 r / min for 2 h to deposit Fe 0 Porphyrin-loaded WO particles 3 The surface was centrifuged, and the precipitate obtained by centrifugation was washed with deionized water, dried in a vacuum drying oven at 60°C, and then ground to obtain a composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide. Labeled as Por-Fe 0 @WO 3 -5, including porphyrin, Fe 0 with WO 3 The mass ratio is 0.1g:0.552g:1g.
[0072] Comparative Example 1
[0073] In this comparative example, the material was prepared in the same manner as in Example 4, except that the loading of porphyrin was omitted, that is, steps (2) and (3) were omitted, and in step (4), WO was directly used as the substrate. 3 Dispersion A replaces porphyrin loaded WO 3 Solution C, the obtained material is marked as Fe 0 @WO 3 .
[0074] Comparative Example 2
[0075] In this comparative example, the material is prepared in the same manner as in Example 4, except that the loading of zero-valent iron is omitted, that is, step (4) and the addition of sodium borohydride are omitted, and in step (5), porphyrin is directly loaded with WO 3 Solution C was centrifuged to obtain a material labeled Por@WO 3 .
[0076] Structural Characterization and Analysis of Porphyrin and Zero-Valent Iron Co-loaded Tungsten Trioxide Composite Materials
[0077] Figure 1 Por-Fe prepared in Example 4 0 @WO 3 -4 transmission electron microscope (TEM). It can be seen that Fe0 The particles appear as darker small particles and are evenly distributed on the WO 3 The surface of Fe 0 The density of the FeO2 is higher, and it usually shows higher contrast in TEM images, presenting darker particles, indicating successful loading. Porphyrins are a class of organic molecules with lighter atoms (such as carbon, hydrogen, nitrogen, etc.) that do not have high electron density like metals or metal oxides. Therefore, porphyrins do not appear as FeO2 in TEM images. 0 or WO 3 Such a stark contrast.
[0078] Figure 2 Por-Fe prepared in Example 4 0 @WO 3 -4 X-ray diffraction spectrum (XRD). It can be seen that Por-Fe 0 @WO 3 The main components of -4 include WO 3 , Fe 0 There are several clear and sharp peaks at about 23°, 24°, 26°, 34°, 42°, and 49°, indicating that WO 3 It exists in a highly crystalline form. At about 44.6° of 2θ, Fe 0 The characteristic peaks of the material indicate that the metal iron particles are successfully loaded in the material, which plays an important role in the redox reaction and phosphate removal of the material. The characteristic of porphyrin appears at about 10° of 2θ, in the form of a wider peak, indicating that it exists in an amorphous state or in a molecular adsorption form.
[0079] Experimental study on phosphorus removal from water by using porphyrin and zero-valent iron co-loaded tungsten trioxide composite material
[0080] 1. Phosphorus removal test of single phosphate body
[0081] Test method: 0.03g of material sample was added into 100mL of aqueous solution sample (the solute only contained 10mg / L NaH 2 PO 4 ) in a conical flask, adjust the pH value of the solution to 7.0 with 0.1mmol / L sodium hydroxide and / or hydrochloric acid solution, then place the conical flask in a constant temperature oscillator, set the temperature to 25°C, and the oscillation rate to 150rpm. At different time points (5, 15, 30, 45, 60min), samples were taken and filtered, and the supernatant was collected. The residual concentration of phosphate was determined using a UV-visible spectrophotometer. The effluent water quality is shown in Table 1.
[0082] Table 1
[0083] Composite Materials Initial total phosphorus concentration Total phosphorus concentration after 60 minutes Total phosphorus removal rate <![CDATA[Por-Fe 0 @WHERE 3 -1]]> 10mg / L 1.4mg / L 86% <![CDATA[Por-Fe 0 @WHERE 3 -2]]> 10mg / L 2.6mg / L 74% <![CDATA[Por-Fe 0 @WHERE 3 -3]]> 10mg / L 1.9mg / L 81% <![CDATA[Por-Fe 0 @WHERE 3 -4]]> 10mg / L 0.1mg / L 99% <![CDATA[Por-Fe 0 @WHERE 3 -5]]> 10mg / L 0.5mg / L 95% <![CDATA[Fe 0 @WHERE 3 ]]> 10mg / L 3.5mg / L 65% <![CDATA[Por@WO 3 ]]> 10mg / L 6.2mg / L 38%
[0084] Experimental conclusion: Por-Fe prepared in Example 4 0 @WO 3 -4 has the best phosphorus removal efficiency, indicating that Por-Fe 0 @WO 3 -4 Fe 0 The amount of porphyrin is in the best ratio, which will not cause Fe 0 A self-catalytic reaction occurs without introducing too many side reactions, while maintaining the highest phosphorus removal efficiency.
[0085] Por-Fe prepared in Example 1 0 @WO 3 -1 phosphorus removal rate is 86%. Compared with Por-Fe 0 @WO3-4,Fe 0 The content of Por-Fe prepared in Example 2 is low, resulting in a slow chemical reaction, thereby reducing the phosphorus removal efficiency. 0 @WO 3 -2 has the lowest phosphorus removal rate, only 74%. 3 Phosphate ions in solution are captured mainly by physical adsorption, while Fe 0 Phosphates are converted into insoluble iron phosphate precipitates mainly through chemical reactions. 3 When the content of Por-Fe increases, the adsorption effect becomes dominant, while the proportion of chemical reaction decreases relatively. This imbalance between adsorption and reaction leads to a decrease in phosphorus removal efficiency. 0 @WO 3 -3 phosphorus removal rate was 81%. Although the amount of porphyrin increased, Fe 0 The amount of ferroporphyrin is still low, resulting in its catalytic effect not being fully exerted, and the efficiency of chemical phosphorus removal is still limited. In addition, iron porphyrin is a complex organic metal complex that can react with Fe 0 The surface interacts, thus affecting the Fe 0 When the amount of iron porphyrin is too high, it may over-cover the Fe 0 surface, reducing Fe 0 direct contact area with phosphate. This over-covering effect will hinder the Fe 0 The reaction between Fe and phosphate reduces the efficiency of chemical phosphorus removal. 0 It plays a key role in phosphorus removal and continues to increase Fe 0 In Example 5, Por-Fe 0 @WO 3 -5 composite material, but the phosphorus removal rate is lower than that of Por-Fe 0 @WO 3-4 decreased, which is mainly due to the phosphorus removal reaction in Fe 0 occurs at the solid-liquid interface. 0 When the amount of Fe is too high, the reaction sites on the solid-liquid interface may reach saturation. 0 The amount of Fe does not effectively increase the active surface area because the reaction rate is limited by the phosphate concentration and diffusion rate at the interface. 0 In the presence of Fe 0 It not only reacts with phosphate, but also with the generated Fe 2+ A self-catalytic reaction occurs to generate magnetite (Fe 3 O 4 ) and other byproducts. These side reactions consume Fe 0 , and reduces its direct reaction with phosphate, thereby reducing the overall phosphorus removal efficiency.
[0086] The above data show that Fe 0 The optimal ratio of Por-Fe to porphyrin is crucial for phosphorus removal efficiency. 0 @WO 3 -4's high efficiency (99% removal rate) indicates that the appropriate amount of Fe 0 Combining the right porphyrin can provide the best chemical reaction efficiency and phosphorus removal effect. 0 When the content is low (such as Por-Fe 0 @WO 3 -1. Por-Fe 0 @WO 3 -3), the chemical reaction is not sufficient, resulting in a decrease in phosphorus removal efficiency; when WO 3 When the content is high (such as Por-Fe 0 @WO 3 -2), although the adsorption effect is enhanced, the reaction is not sufficient, resulting in the lowest phosphorus removal rate. 0 Excess (such as Por-Fe 0 @WO 3 -5), the phosphorus removal efficiency slightly decreased due to adsorption site saturation or autocatalytic effect.
[0087] Fe of Comparative Example 1 0 @WO 3 The total phosphorus removal rate was 65% (without porphyrin loading), which was significantly lower than that of Por-Fe 0 @WO 3 -4. This is due to the lack of porphyrin, which reduces the electron transfer efficiency of the composite material and leads to Fe 0 The oxidation efficiency of Fe 2+ and Fe 3+The generation of Por@WO in Comparative Example 2 is insufficient, thereby reducing the reaction rate with phosphate and the removal effect of phosphate. 3 (Omitting the zero-valent iron load) the total phosphorus removal rate was only 38%, the lowest among all samples. 0 After that, no iron phosphate precipitation can be generated in the system, and phosphate removal depends only on porphyrin and WO 3 This indicates that Fe 0 The above results show that porphyrin and Fe 0 Porphyrin plays an important role in the phosphorus removal process. Porphyrin enhances Fe 2+ and Fe 3+ The formation of Fe 0 Ensure that Fe in the system 2+ and Fe 3+ Source.
[0088] 2. Phosphorus removal test in water in the presence of competitive ions
[0089] Test method: 0.03 g of material sample was added into 100 mL of aqueous solution sample (the solute contained NaH 2 PO 4 , concentration 10mg / L Na 2 SO 4 , NaCl at 10 mg / L, and NaNO at 10 mg / L 3 ) in a conical flask, adjust the pH value of the solution to 7.0 with 0.1mmol / L sodium hydroxide and / or hydrochloric acid solution, then place the conical flask in a constant temperature oscillator, set the temperature to 25°C, and the oscillation rate to 150rpm. At different time points (5, 15, 30, 45, 60min), samples were taken and filtered, and the supernatant was collected. The residual concentration of phosphate was determined using a UV-visible spectrophotometer. The effluent water quality is shown in Table 2.
[0090] Table 2
[0091] Composite Materials Initial total phosphorus concentration Total phosphorus concentration after 60 minutes Total phosphorus removal rate <![CDATA[Por-Fe 0 @WHERE 3 -4]]> 10mg / L 0.3mg / L 97% <![CDATA[Fe 0 @WHERE 3 ]]> 10mg / L 6.0mg / L 40% <![CDATA[Por@WO 3 ]]> 10mg / L 6.3mg / L 37%
[0092] It can be seen that Por-Fe 0 @WO 3 -4 still has a very efficient phosphate removal ability in the presence of competing ions. By comparison with the comparative example, the total phosphorus removal rate of comparative example 1 was reduced from 65% to 40% due to the lack of porphyrin, while the removal rate of comparative example 2 did not change significantly, which shows that porphyrin plays a key role in the selective adsorption of phosphate. Although the material lacking porphyrin still has a certain removal effect, it is greatly affected by competitive ions due to its poor selectivity.
[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide, characterized in that: The following steps are involved: (1) adding WO3 powder to deionized water, then purging with nitrogen to remove dissolved oxygen, and then performing ultrasonic dispersion treatment to obtain WO3 dispersion A; (2) dissolving porphyrin in an organic solvent to obtain a porphyrin solution B; (3) under stirring conditions, adding the porphyrin solution B to the WO3 dispersion A, then performing ultrasonic dispersion treatment, and then stirring treatment to obtain a porphyrin-loaded WO3 solution C; (4) adding iron salt to the porphyrin-loaded WO3 solution C, and then stirring to obtain a mixed solution D; (5) Adding a reducing agent to the mixed solution D, stirring the mixed solution, and then centrifuging the mixed solution. Washing, drying, and grinding the precipitate obtained by centrifugation to obtain the porphyrin and zero-valent iron co-loaded tungsten trioxide composite material.
2. The method for preparing the composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide according to claim 1, characterized in that: In step (1), the material-liquid ratio of the WO3 powder to deionized water is 0.5-3 g: 100-500 mL.
3. The method for preparing the composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide as claimed in claim 1, characterized in that: In step (2), the organic solvent is any one of ethanol, dichloromethane, N,N-dimethylformamide, dimethyl sulfoxide or tetrahydrofuran, or a mixture of two or more thereof in any proportion; the porphyrin is any one of iron porphyrin, zinc porphyrin, cobalt porphyrin or nickel porphyrin, or a mixture of two or more thereof in any proportion, and the solid-liquid ratio of the porphyrin to the organic solvent is 0.05-2 g:50-500 mL.
4. The method for preparing the composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide according to claim 1, characterized in that: In step (3), the dosage ratio of the WO3 dispersion A and the porphyrin solution B is: based on the porphyrin and WO3 powder contained, the mass ratio of porphyrin to WO3 powder is 0.1-0.2:1-1.
5.
5. The method for preparing the composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide as claimed in claim 1, characterized in that: In step (4), the iron salt is any one of FeSO4, FeCl3 or Fe(NO3)3 or a mixture of two or more thereof in any proportion, and the dosage ratio of the iron salt and porphyrin-loaded WO3 solution C is: based on the iron element contained and the WO3 powder, the mass ratio of the iron element to the WO3 powder is 0.1-15g:0.5-30g.
6. The method for preparing the composite material of porphyrin and zero-valent iron co-loaded with tungsten trioxide as claimed in claim 1, characterized in that: In step (5), the reducing agent is any one of sodium borohydride, potassium borohydride, vitamin C, hydroxylamine hydrochloride, tea polyphenols, and ascorbic acid, or a mixture of two or more of them in any proportion, and the mass ratio of the reducing agent to the iron salt is 0.1-5g:0.1-10g.
7. A porphyrin and zero-valent iron co-loaded tungsten trioxide composite material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the porphyrin and zero-valent iron co-loaded tungsten trioxide composite material as claimed in claim 7 in phosphorus removal from water.
9. A method for removing phosphate from water, characterized in that: The method comprises the following steps: adding the porphyrin and zero-valent iron co-loaded tungsten trioxide composite material as claimed in claim 7 into a phosphate-containing water body, and stirring the reaction at room temperature.
10. The method for removing phosphate from water according to claim 9, characterized in that: The phosphate concentration of the water body is controlled at 0.1-100 mg / L, the dosage of the composite material is 0.1-5.0 g / L, the reaction conditions are pH value 5-10, stirring speed 50-300 r / min, and reaction time 30-120 min.
Citation Information
Patent Citations
Composite dephosphorization adsorbent and method for dephosphorization in water body
CN108993444A
Bagasse-loaded zero-valent iron adsorbent, and preparation method and application thereof
CN110314655A
Domestic sewage treatment agent capable of efficiently removing phosphorus and preparation method thereof
CN113603256A
Preparation method and application of carbon nanotube loaded metalloporphyrin molecular catalyst
CN117619443A
Method for producing magnesium porphyrin complex
JP2004292344A