Preparation method and application of graphene aerogel-based imprinted adsorption material
A graphene aerogel-based imprinted adsorption material addresses the limitations of existing adsorption materials by achieving high quinoline removal capacity and selectivity, with efficient recovery and regeneration capabilities.
Patent Information
- Application Number
- CN202411241852.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
AI Technical Summary
Existing adsorption materials for quinoline removal in coking wastewater suffer from poor adsorption performance, non-selectivity, and difficult recovery, limiting their effectiveness in separation and recovery of quinoline.
A graphene aerogel-based imprinted adsorption material is prepared by forming a complex with quinoline and a functional monomer, followed by polymerization and removal of the template molecule, resulting in a material with high selectivity and ease of recovery.
The material exhibits a high adsorption capacity, selectivity, and cyclic regeneration ability, effectively removing quinoline from coking wastewater while maintaining structural integrity.
Smart Images

Figure CN119075938A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment adsorption materials, and specifically relates to a preparation method and application of a graphene aerogel-based imprinted adsorption material. Background Art
[0002] Coking wastewater is a typical industrial organic wastewater, mainly from the coking and gas purification process. It is composed of organic substances such as phenols, quinoline, pyridine and polycyclic aromatic hydrocarbons, and has the characteristics of large discharge volume, high pollutant concentration, strong toxicity and difficulty in degradation. Biological methods are widely used in the treatment of coking wastewater due to their advantages such as large treatment capacity and no secondary pollution. However, quinoline, as a typical difficult-to-degrade organic pollutant in coking wastewater, still has a high content in the biological treatment effluent of coking wastewater. If it cannot be thoroughly and effectively treated, direct discharge will endanger human health and the ecological environment. However, if it is recycled, it is an important chemical that can be used as an intermediate in printing and dyeing, medicine, optoelectronics and other fields, and has an economic value that cannot be underestimated. Therefore, it is of great significance to find a way to remove quinoline from coking wastewater efficiently, selectively and non-destructively, and to realize the resource recovery and utilization of quinoline while cleaning coking wastewater.
[0003] The adsorption method is the most widely used method due to its simple operation, high efficiency and relatively mild reaction conditions. However, the existing adsorption materials have problems such as poor adsorption performance, non-selectivity and difficulty in recovery when used for quinoline removal, which have certain limitations for the separation and recovery of quinoline in coking wastewater. Wang et al. (Processes, 2020, 8: 156–170.) studied the adsorption of quinoline by coke powder, which was only 1.38 mg·g -1 , and the powder adsorbent dissolves severely after adsorption, which is easy to cause secondary pollution. Kang et al. (Chemical Engineering Journal, 2021, 412: 128686.) prepared three-dimensional amino-functionalized graphene aerogel for adsorbing quinoline in water, with a saturated adsorption capacity of 103 mg·g -1 , and after adsorption saturation, the block graphene aerogel can be quickly and non-destructively separated and recovered from the liquid phase, but it has no specific recognition for the adsorption of quinoline. Cui et al. (Chemical Engineering Journal, 2020, 397: 125480.) used magnetic carbon nanospheres as carriers and acrylamide as functional monomers to prepare a magnetically responsive imprinted adsorption material, which achieved selective adsorption of quinoline with an equilibrium adsorption capacity of 76.63 mg g -1 , can be separated and recovered with the help of an external magnetic field, but the introduction of magnetic particles will cause the adsorbent to agglomerate, affecting the dispersion and adsorption of the adsorbent in the liquid phase. Summary of the invention
[0004] The main purpose of the present invention is to overcome the deficiencies in the prior art and solve the technical problems of poor adsorption performance, non-selectivity and difficult recovery of existing adsorption materials when used for quinoline removal. The present invention provides a preparation method of a graphene aerogel-based imprinted adsorption material and its application.
[0005] The design concept of the present invention is: Graphene aerogel has a large specific surface area, developed pores, rich active sites, easy functionalization and excellent mechanical properties. As a carrier, it helps to generate as many effective imprinting sites as possible during the imprinting process, while achieving rapid mass transfer. In addition, the three-dimensional block graphene aerogel has obvious advantages in solid-liquid separation, making it easy to separate and recover the prepared imprinted material from the liquid phase after adsorption saturation. Therefore, the present invention uses graphene aerogel as a carrier, and the template molecule quinoline and the functional monomer 4-vinylbenzoic acid produce complementary interactions to form a complex, and by adding a cross-linking agent and an initiator, an imprinting polymerization reaction is carried out around the complex, and then the template molecule quinoline in the polymer is removed to obtain a graphene aerogel-based imprinted adsorption material.
[0006] The present invention is implemented by the following technical scheme: A method for preparing a graphene aerogel-based imprinted adsorption material, comprising the following steps: S1. First, a graphene oxide (carbon precursor, prepared by modified Hummers method with graphite powder, sodium nitrate and potassium permanganate as raw materials) aqueous solution with a concentration of 3 mg / mL to 5 mg / mL is used as a raw material, and ammonium citrate as a reducing agent is added. Selecting ammonium citrate as a reducing agent can significantly improve the structural stability, hydrophilicity and adsorption performance of graphene aerogel. The mass ratio of ammonium citrate to graphene oxide is (3 to 7):1. The graphene hydrogel is prepared by hydrothermal reaction at a temperature of 100°C to 150°C for 9h to 12h; then, the graphene hydrogel is dialyzed with an ethanol aqueous solution for 24h to 48h; finally, the graphene aerogel is prepared by freeze drying at a temperature of -86°C for 2d to 3d for subsequent use; S2, add template molecule quinoline and functional monomer 4-vinylbenzoic acid to acetonitrile solvent, the amount of acetonitrile solvent added is 1200~2000 times the mass of graphene aerogel prepared in step S1, the amount of template molecule quinoline added is 10~20 times the mass of graphene aerogel prepared in step S1, the amount of functional monomer added is 2~5 times the mass of template molecule quinoline, ultrasonic treatment for 10min~20min, and then prepolymerize under magnetic stirring at 25°C for 0.5h~4h to obtain a prepolymer solution for The function of the functional monomer is to interact with the template molecule quinoline through its own active functional group to form an imprinted hole that matches quinoline in terms of stereo configuration and affinity, so as to achieve the effect of specifically recognizing and adsorbing quinoline. The functional monomer preferably contains an acidic functional group and an aromatic ring, which can interact with the template molecule quinoline through hydrogen bonding, acid-base interaction or Π-Π conjugation. The cross-linking agent can form a high molecular rigid polymer around the functional monomer-template molecule prepolymer, thereby fixing the imprinted recognition site; S3. First, add a crosslinking agent, an initiator and the graphene aerogel prepared in step S1 to the prepolymer solution prepared in step S2, wherein the amount of the crosslinking agent added is 0.5-0.8 times the mass of the functional monomer added in step S2, and the amount of the initiator added is 0.005-0.015 times the mass of the functional monomer added in step S2, and perform ultrasonic treatment for 10-20 minutes; then, purge with an inert gas for 10-20 minutes to remove the oxygen dissolved in the reaction solution, and the preferred inert gas is nitrogen; finally, perform an imprinting polymerization reaction at a temperature of 60-70°C for 10-24 hours to obtain an imprinted polymer layer; S4, eluting the imprinted polymer layer prepared in step S3 with a methanol / acetic acid mixed solution to remove the template molecule quinoline in the imprinted polymer layer, and then combining with a UV-visible spectrophotometer to ensure that the template molecule is completely removed; then freeze-drying at a temperature of -86°C for 2d~3d to obtain a graphene aerogel-based imprinted adsorption material; the freeze-drying method can minimize the damage of water to the pore structure, slowly open the pores, and retain the pore structure.
[0007] The graphene aerogel-based imprinted adsorption material prepared by the above method of the present invention is a three-dimensional black block, showing a cross-linked network structure. After being compressed with a 100 g weight, the graphene aerogel-based imprinted material did not suffer structural damage and recovered to its original height, showing excellent structural stability. The adsorption test showed that the saturated adsorption capacity of quinoline in aqueous solution by the graphene aerogel-based imprinted material was 88.25 mg·g -1 , the adsorption equilibrium can be reached within 6 h, and it also exhibits excellent quinoline selective adsorption capacity and cyclic regeneration ability.
[0008] Furthermore, in the step S1, the hydrothermal reaction is carried out in an electric heated forced air drying oven.
[0009] Furthermore, in step S1, the volume fraction of the ethanol aqueous solution is 10% to 20%.
[0010] Furthermore, in the step S3, the cross-linking agent is ethylene glycol dimethacrylate, divinylbenzene or ethyl methacrylate.
[0011] Furthermore, in the step S3, the initiator is azobisisobutyronitrile or azobisisoheptanenitrile.
[0012] Furthermore, in step S4, the volume ratio of the methanol solution to the acetic acid solution in the methanol / acetic acid mixed solution is (8-10):1.
[0013] Application of the graphene aerogel-based imprinted adsorption material prepared by the preparation method as described above: The graphene aerogel-based imprinted adsorption material is used for the adsorption and separation of quinoline molecules in coking wastewater. The blocky graphene aerogel-based imprinted adsorption material exhibits a large adsorption capacity, high selectivity and good regeneration performance for quinoline molecules, and has obvious solid-liquid separation advantages, and can achieve fast and convenient separation and recovery.
[0014] The beneficial effects of the present invention are: The graphene aerogel-based imprinted adsorption material prepared by the present invention has strong adsorption capacity, high selectivity, good reusability and convenient separation and recovery characteristics, can efficiently, deeply and non-destructively remove quinoline from coking wastewater, has strong practicality, and can be widely used in detection, adsorption, separation and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 is a physical picture of the graphene aerogel-based imprinted material prepared in Example 1; Figure 2 is a scanning electron microscope morphology image of the graphene aerogel-based imprinted material prepared in Example 1; Figure 3 is a macroscopic compressibility test graph of the graphene aerogel-based imprinted material prepared in Example 1; Figure 4 is the kinetic fitting curve of the graphene aerogel-based imprinting material prepared in Example 1; Figure 5 is the isothermal fitting curve of the graphene aerogel-based imprinted material prepared in Example 1; Figure 6 is a test graph of the regeneration performance of the graphene aerogel-based imprinted material prepared in Example 1; Figure 7 are the adsorption kinetic curves of the products of Example 1 and Comparative Example 1; Figure 8 It is the adsorption selectivity test graph of the products of Example 1 and Comparative Example 1; Fig. 9 This is a physical picture of the product of Comparative Example 2. DETAILED DESCRIPTION
[0016] The following embodiments are only preferred technical solutions of the present invention and are not intended to limit the present invention in any way. For those skilled in the art, the present invention may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should all be included in the protection scope of the present invention. Example 1
[0017] A method for preparing a graphene aerogel-based imprinted adsorption material, characterized in that it comprises the following steps: S1. First, 5 mL of 3 mg / mL graphene oxide aqueous solution was measured as a raw material, 60 mg of reducing agent ammonium citrate was added, and a hydrothermal reaction was performed at 120°C for 10 h to obtain a graphene hydrogel; then, the solution was dialyzed with an ethanol aqueous solution for 48 h; finally, the solution was freeze-dried at -86°C for 2 days to obtain a graphene aerogel for subsequent use; S2, add 236 µL of template molecule quinoline and 0.889 g of functional monomer 4-vinylbenzoic acid into 20 mL of acetonitrile solvent, ultrasonically treat for 20 min, and then prepolymerize under magnetic stirring at 25 °C for 2 h to obtain a prepolymer solution for use in the next step; S3. First, add 422 μL of ethylene glycol dimethacrylate, 0.0089 g of azobisisobutyronitrile and 0.01 g of graphene aerogel prepared in step S1 to the prepolymer solution prepared in step S2, and perform ultrasonic treatment for 20 min; then, purge with nitrogen for 10 min; finally, perform imprinting polymerization reaction at 60° C. for 10 h to obtain an imprinted polymer layer; S4. The imprinted polymer layer prepared in step S3 is eluted with a methanol / acetic acid mixed solution (volume ratio 9:1) to remove the template molecule quinoline in the imprinted polymer layer, and then freeze-dried at -86°C for 2 days to obtain a graphene aerogel-based imprinted adsorption material.
[0018] Figure 1 The macroscopic photo of the graphene aerogel-based imprinted adsorbent is shown in Figure 1. It can be seen from the figure that the graphene aerogel-based imprinted adsorbent is a three-dimensional black cylindrical material with a cross-sectional diameter of 1.8 cm and a height of 1.5 cm. The block graphene aerogel-based imprinted adsorbent has excellent solid-liquid separation advantages and can be easily separated and recovered from the liquid phase after adsorption saturation.
[0019] Figure 2Shown is the scanning electron microscope morphology of the graphene aerogel-based imprinted adsorption material. It can be seen that the graphene aerogel-based imprinted adsorption material presents a mutually cross-linked network structure with developed pores, which can provide sufficient adsorption space and abundant adsorption sites during the adsorption process, which is beneficial to the adsorption of quinoline.
[0020] Figure 3 The figure shows the macroscopic compression test diagram of the graphene aerogel-based imprinted adsorbent material. The graphene aerogel-based imprinted adsorbent material was compressed with a 100 g weight. After removing the weight, the graphene aerogel-based imprinted adsorbent material did not suffer obvious structural damage and recovered to its original height, indicating that the graphene aerogel-based imprinted adsorbent material has good structural stability.
[0021] Figure 4 The figure shows the adsorption kinetics fitting curve of the graphene aerogel-based imprinted adsorbent. As can be seen from the figure, the adsorption rate of quinoline on the graphene aerogel-based imprinted adsorbent changes from fast to slow over time, and the adsorption equilibrium is reached in 6 hours, with an equilibrium adsorption capacity of 63.14 mg·g -1 The adsorption data were fitted and analyzed using pseudo-first-order kinetic model and pseudo-second-order kinetic model. The pseudo-first-order correlation coefficient R 2 (0.9608) is less than the quasi-secondary correlation coefficient R 2 (0.9779), indicating that the quasi-second-order kinetic model can better fit the adsorption results, and the adsorption process of quinoline by graphene aerogel-based imprinted adsorption material shows adsorption characteristics similar to chemical adsorption.
[0022] Figure 5 The adsorption isotherm fitting curve of the graphene aerogel-based imprinted adsorption material is shown. It can be seen that with the increase of the initial concentration, the adsorption amount of quinoline by the graphene aerogel-based imprinted adsorption material increases until the adsorption is saturated, and the saturated adsorption amount is 88.25 mg g -1 The isotherm adsorption data were further fitted using the Langmuir isotherm model and the Friedrich isotherm model, and the correlation coefficient R 2 (0.98) is greater than the correlation coefficient R of the Friedrich isotherm model 2 (0.9028), indicating that the Langmuir isotherm model has a higher fit with the isothermal adsorption results. The adsorption of quinoline by the graphene aerogel-based imprinted adsorption material is mainly a monolayer adsorption on a uniform surface. This is due to the presence of uniform imprinted pores on the surface of the graphene aerogel-based imprinted adsorption material.
[0023] Figure 6Shown is the adsorption regeneration performance test chart of the graphene aerogel-based imprinted adsorbent material. After 5 adsorption and desorption cycles, the adsorption amount of quinoline by the graphene aerogel-based imprinted adsorbent material still reaches 90% of the initial adsorption amount, indicating that the graphene aerogel-based imprinted adsorbent material exhibits excellent cyclic regeneration ability as an adsorbent. Example 2
[0024] A method for preparing a graphene aerogel-based imprinted adsorption material, characterized in that it comprises the following steps: S1. First, 5 mL of 3 mg / mL graphene oxide aqueous solution was measured as a raw material, 60 mg of reducing agent ammonium citrate was added, and a hydrothermal reaction was performed at 120°C for 11 h to obtain a graphene hydrogel; then, the solution was dialyzed with an ethanol aqueous solution for 48 h; finally, the solution was freeze-dried at -86°C for 2 days to obtain a graphene aerogel for subsequent use; S2, add 236 µL of template molecule quinoline and 0.889 g of functional monomer 4-vinylbenzoic acid into 20 mL of acetonitrile solvent, ultrasonically treat for 10 min, and then prepolymerize under magnetic stirring at 25 °C for 0.5 h to obtain a prepolymer solution for use in the next step; S3. First, add 422 μL of ethylene glycol dimethacrylate, 0.0065 g of azobisisobutyronitrile and 0.01 g of the graphene aerogel prepared in step S1 to the prepolymer solution prepared in step S2, and perform ultrasonic treatment for 20 min; then, purge with nitrogen for 10 min; finally, perform imprinting polymerization reaction at 60° C. for 12 h to obtain an imprinted polymer layer; S4, eluting the imprinted polymer layer prepared in step S3 with a methanol / acetic acid mixed solution (volume ratio 9:1) to remove the template molecule quinoline in the imprinted polymer layer, and then freeze-drying it at -86°C for 2 days to obtain a graphene aerogel-based imprinted adsorption material, whose saturated adsorption capacity for quinoline is 80.19 mg·g -1 , which has the ability to selectively recognize and adsorb quinoline. Example 3
[0025] A method for preparing a graphene aerogel-based imprinted adsorption material, characterized in that it comprises the following steps: S1. First, 5 mL of 3 mg / mL graphene oxide aqueous solution was measured as a raw material, 65 mg of reducing agent ammonium citrate was added, and a hydrothermal reaction was performed at 130°C for 9 h to obtain a graphene hydrogel; then, the solution was dialyzed with an ethanol aqueous solution for 48 h; finally, the solution was freeze-dried at -86°C for 2 d to obtain a graphene aerogel for subsequent use; S2, add 236 µL of template molecule quinoline and 0.889 g of functional monomer 4-vinylbenzoic acid into 20 mL of acetonitrile solvent, ultrasonically treat for 20 min, and then prepolymerize under magnetic stirring at 25 °C for 1 h to obtain a prepolymer solution for use in the next step; S3. First, add 422 μL of ethylene glycol dimethacrylate, 0.0089 g of azobisisobutyronitrile and 0.01 g of graphene aerogel prepared in step S1 to the prepolymer solution prepared in step S2, and perform ultrasonic treatment for 20 min; then, purge with nitrogen for 10 min; finally, perform imprinting polymerization reaction at 65° C. for 11 h to obtain an imprinted polymer layer; S4, eluting the imprinted polymer layer prepared in step S3 with a methanol / acetic acid mixed solution (volume ratio 9:1) to remove the template molecule quinoline in the imprinted polymer layer, and then freeze-drying it at -86°C for 2 days to obtain a graphene aerogel-based imprinted adsorption material, whose saturated adsorption capacity for quinoline is 77.46 mg g -1 , which has the ability to selectively recognize and adsorb quinoline.
[0026] Comparative Example 1
[0027] 60 mg of ammonium citrate was added to 5 mL of 3 mg / mL graphene oxide aqueous solution, and the hydrothermal reaction was carried out at 120°C for 10 h to form graphene hydrogel. After dialyzed with ethanol aqueous solution for 48 h, the graphene aerogel was obtained by freeze-drying at -86°C for 2 d.
[0028] The performance of the graphene aerogel-based imprinted adsorption material prepared in Example 1 was compared with that of the non-imprinted graphene aerogel prepared in Comparative Example 1. Figure 7 and Figure 8 The adsorption kinetics curves and selectivity test diagrams of the two are shown respectively. It can be seen that the adsorption capacity of quinoline by the unimprinted graphene aerogel and the graphene aerogel-based imprinted adsorption material is 31.25 mg·g -1 and 63.14 mg·g -1 , due to the presence of a large number of imprinted holes on the surface of the imprinted material, the adsorption performance is significantly improved. Phenol and pyridine, which have high content and similar structure in coking wastewater, were selected as interfering molecules, and a mixed solution of the three was prepared to test the selective recognition adsorption ability of the material. As can be seen from the figure, the graphene aerogel-based imprinted adsorption material prepared in Example 1 has a high selective adsorption capacity for quinoline, which is beneficial to the lossless removal and enrichment and recycling of quinoline in wastewater.
[0029] Comparative Example 2
[0030] 60 mg of ammonium citrate was added to 5 mL of 3 mg / mL graphene oxide aqueous solution, and the hydrothermal reaction was carried out at 160°C for 15 h to form graphene hydrogel, which was dialyzed with ethanol aqueous solution for 48 h and then freeze-dried at -86°C for 2 d to obtain graphene aerogel. Then, 236 μL of quinoline and 0.889 g of 4-vinylbenzoic acid were added to 20 mL of acetonitrile solvent, and after ultrasonication for 20 min, magnetic stirring was used for prepolymerization at 25°C for 4 h. Then, 0.01 g of graphene aerogel, 422 μL of ethylene glycol dimethacrylate and 0.0089 g of azobisisobutyronitrile were added, and after ultrasonication for 20 min, nitrogen was purged for 10 min, and imprinting polymerization was carried out at 60°C for 18 h. Quinoline was eluted with a methanol / acetic acid mixed solution (volume ratio 9:1), and the mixture was freeze-dried at -86°C for 2 h. d, the graphene aerogel-based imprinted adsorption material was obtained, and its saturated adsorption capacity for quinoline was 35.46 mg g -1 , the effect of selective adsorption of quinoline is poor.
[0031] Fig. 9 The picture shown is a physical picture of the product of Comparative Example 2. It can be seen that the surface of the synthesized graphene aerogel-based imprinted adsorption material is severely wrinkled, irregular in shape, and relatively brittle.
[0032] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A method for preparing a graphene aerogel-based imprinted adsorption material, It is characterized in that The following steps are involved: S1. First, a graphene oxide aqueous solution with a concentration of 3 mg / mL to 5 mg / mL is used as a raw material, and a reducing agent ammonium citrate is added, and the mass ratio of ammonium citrate to graphene oxide is (3 to 7):
1. The graphene hydrogel is prepared by hydrothermal reaction at a temperature of 100°C to 150°C for 9h to 12h; then, the graphene hydrogel is dialyzed with an ethanol aqueous solution for 24h to 48h; finally, the graphene aerogel is prepared by freeze drying at a temperature of -86°C for 2d to 3d, and then, the graphene aerogel is prepared for use in the subsequent step; S2, adding the template molecule quinoline and the functional monomer 4-vinylbenzoic acid to the acetonitrile solvent, wherein the amount of the acetonitrile solvent added is 1200-2000 times the mass of the graphene aerogel prepared in step S1, the amount of the template molecule quinoline added is 10-20 times the mass of the graphene aerogel prepared in step S1, and the amount of the functional monomer added is 2-5 times the mass of the template molecule quinoline, ultrasonic treatment for 10-20 minutes, and then prepolymerization under magnetic stirring at 25° C. for 0.5-4 hours to obtain a prepolymer solution for use in the subsequent step; S3. First, add a crosslinking agent, an initiator and the graphene aerogel prepared in step S1 to the prepolymer solution prepared in step S2, wherein the amount of the crosslinking agent added is 0.5-0.8 times the mass of the functional monomer added in step S2, and the amount of the initiator added is 0.005-0.015 times the mass of the functional monomer added in step S2, and perform ultrasonic treatment for 10-20 minutes; then, purge with inert gas for 10-20 minutes; finally, perform imprinting polymerization reaction at a temperature of 60-70°C for 10-24 hours to obtain an imprinted polymer layer; S4, eluting the imprinted polymer layer prepared in step S3 with a methanol / acetic acid mixed solution to remove the template molecule quinoline in the imprinted polymer layer, and then freeze-drying it at -86°C for 2d~3d to obtain a graphene aerogel-based imprinted adsorption material.
2. A method for preparing a graphene aerogel-based imprinted adsorption material according to claim 1, It is characterized in that In the step S1, the hydrothermal reaction is carried out in an electric heated forced air drying oven.
3. A method for preparing a graphene aerogel-based imprinted adsorption material according to claim 1, It is characterized in that In step S1, the volume fraction of the ethanol aqueous solution is 10% to 20%.
4. The method for preparing a graphene aerogel-based imprinted adsorption material according to claim 1, It is characterized in that In the step S3, the cross-linking agent is ethylene glycol dimethacrylate, divinylbenzene or ethyl methacrylate.
5. The method for preparing a graphene aerogel-based imprinted adsorption material according to claim 1, It is characterized in that In the step S3, the initiator is azobisisobutyronitrile or azobisisoheptanenitrile.
6. A method for preparing a graphene aerogel-based imprinted adsorption material according to claim 1, It is characterized in that In step S4, the volume ratio of the methanol solution to the acetic acid solution in the methanol / acetic acid mixed solution is (8-10):
1.