Super-hydrophobic activated carbon coating material as well as preparation method and application thereof

A cost-effective and durable super hydrophobic activated carbon coating is produced by exposing hydroxyl groups on activated carbon, chemically grafting organosilane, and mixing with a resin binder, addressing the limitations of expensive nano materials and solvent-induced separation in existing technologies, achieving efficient oil-water separation and emulsion demulsification.

CN119075939AActive Publication Date: 2024-12-06SHANDONG UNIV +1

Patent Information

Application Number
CN202411309426.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-06
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

Existing super hydrophobic materials for oil-water separation use expensive nano materials and have complex preparation processes, limiting their large-scale application, and existing methods for modifying activated carbon into super hydrophobic coatings result in poor performance due to solvent-induced separation of the coating from the activated carbon.

Method used

A method involving washing activated carbon to expose hydroxyl groups, reacting it with organosilane in an alkaline system for chemical grafting and polymerization, and mixing with a resin binder to create a super hydrophobic activated carbon coating that is chemically bonded, ensuring durability and performance.

Benefits of technology

The resulting super hydrophobic activated carbon coating is cost-effective, durable, and exhibits excellent hydrophobic properties, suitable for oil-water separation and emulsion demulsification, maintaining performance through various tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075939A_ABST
    Figure CN119075939A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of oil-water separation and emulsion demulsification, and relates to a super-hydrophobic activated carbon coating material as well as a preparation method and application thereof. The preparation method comprises the following steps: cleaning the activated carbon until hydroxyl on the surface of the activated carbon is exposed; the cleaned activated carbon and organosilane react in an alkaline system containing water, so that the organosilane is hydrolyzed and chemically bonded with hydroxyl on the surface of the activated carbon, meanwhile, the organosilane grafted on the surface of the activated carbon is polymerized, and the super-hydrophobic activated carbon is obtained; wherein the alkyl carbon number of the organosilane is not less than 10; and uniformly mixing the super-hydrophobic active carbon and the resin binder in a solvent to obtain the super-hydrophobic active carbon. The coating material prepared from the super-hydrophobic activated carbon has the advantages of low price, firmness, durability, excellent performance, simple preparation process and the like, and can be widely applied to the fields of oil-water separation, emulsion demulsification and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil-water separation and emulsion demulsification, and relates to a super-hydrophobic activated carbon coating material and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] With the rapid development of industry and transportation, the discharge of oily wastewater has continued to rise, posing a serious threat to the ecological environment and human health. Traditional oil-water separation methods, such as gravity separation and natural sedimentation, have defects such as low separation efficiency, long treatment cycle, and easy secondary pollution, which are difficult to meet the growing environmental protection needs. Therefore, the development of efficient and environmentally friendly oil-water separation technology has become the focus of current research.

[0004] Super hydrophobic materials, by virtue of their unique surface properties, show great application potential in the field of oil-water separation and emulsion demulsification. Super hydrophobic materials have the characteristics of static contact angle greater than 150 ° and rolling angle less than 10 °, which can effectively repel water molecules and attract oil molecules at the same time, thereby achieving oil-water separation and emulsion demulsification. In recent years, researchers have prepared super hydrophobic materials by a variety of methods, and applied them to the field of oil-water separation, and achieved remarkable results. However, the inventors have found that in the prior art, most super hydrophobic materials generally use expensive micro-nano materials (such as graphene oxide, carbon nanotubes) to construct surface roughness, for example, the patent of publication number CN117861448A discloses a super hydrophobic oil-water separation membrane prepared by using nano zinc oxide and graphene oxide, which has good oily wastewater treatment efficiency. However, nano zinc oxide and graphene oxide are expensive, and the oil-water separation material preparation process is complicated, which limits its large-scale application. Summary of the invention

[0005] In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a super hydrophobic activated carbon coating material and a preparation method and application thereof. The present invention utilizes super hydrophobic activated carbon to make a coating material, which has the advantages of low price, durability, excellent performance, simple preparation process, etc., and can be widely used in fields such as oil-water separation and emulsion demulsification.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] In a first aspect, a method for preparing a super-hydrophobic activated carbon coating material comprises the following steps:

[0008] The activated carbon is washed until the hydroxyl groups on its surface are exposed;

[0009] The cleaned activated carbon is reacted with an organosilane in an alkaline system containing water, so that the organosilane is hydrolyzed and chemically bonded to the hydroxyl groups on the surface of the activated carbon, and the organosilane grafted on the surface of the activated carbon is polymerized to obtain a super-hydrophobic activated carbon; wherein the carbon number of the alkyl group of the organosilane is not less than 10;

[0010] The super-hydrophobic activated carbon and the resin binder are uniformly mixed in a solvent to obtain the super-hydrophobic activated carbon.

[0011] At present, the methods for modifying activated carbon into hydrophobic / super-hydrophobic activated carbon include: surface passivation, removal of hydrophilic groups, hydrophobic modification of oxide loads, surface group grafting, silicone coating, and nano-coating. Among them, the method for modifying into super-hydrophobic activated carbon is mainly based on coating with silicone coating and nano-coating. However, the coating of super-hydrophobic activated carbon prepared by these methods is mainly compounded in physical ways such as deposition. When it is used as a super-hydrophobic component to prepare a coating material, since a binder needs to be mixed in a solvent, the coating is easily swollen in the solvent, resulting in the separation of the coating and the activated carbon, thereby reducing the super-hydrophobic performance of the prepared coating material, or even having no super-hydrophobic performance. Therefore, it is difficult to directly prepare a super-hydrophobic activated carbon coating material using existing super-hydrophobic activated carbon.

[0012] The present invention exposes the hydroxyl groups on the surface of the activated carbon by washing, and chemically grafts the silanols obtained by hydrolyzing the organic silane with the hydroxyl groups as active sites, so that the surface of the activated carbon is grafted with a hydrophobic long carbon chain with a carbon number of not less than 10, and polymerizes the organic silane with the hydrophobic long carbon chain under alkaline conditions, so that the hydrophobic long carbon chain is firmly fixed on the surface of the activated carbon to form super-hydrophobic activated carbon, and then the super-hydrophobic activated carbon is mixed with a resin binder in a solvent to ensure that the hydrophobic long carbon chain does not fall off the surface of the activated carbon, thereby ensuring the super-hydrophobic performance of the super-hydrophobic activated carbon coating material.

[0013] On the other hand, a super hydrophobic activated carbon coating material is obtained by the above preparation method.

[0014] In a third aspect, a super hydrophobic activated carbon coating is provided, wherein the super hydrophobic activated carbon coating material is attached to the surface of a substrate.

[0015] In a fourth aspect, a use of the above-mentioned superhydrophobic activated carbon coating material or superhydrophobic activated carbon coating in oil-water separation and / or emulsion demulsification.

[0016] The beneficial effects of the present invention are:

[0017] 1. The super-hydrophobic activated carbon coating material prepared by the present invention is obtained by modifying activated carbon with organosilane to obtain super-hydrophobic activated carbon, mixing with epoxy resin solution and then coating on a substrate. There are a large number of hydroxyl groups on the surface of activated carbon. After hydrolysis, organosilane polymerizes on the surface of activated carbon under alkaline conditions, so that a large number of hydrophobic long carbon chains are grafted on the activated carbon, thereby realizing super-hydrophobic modification of activated carbon. The modification method is simple to operate, low in price, and the modified activated carbon has excellent hydrophobic properties.

[0018] 2. The super-hydrophobic activated carbon coating material prepared by the present invention has the advantages of low price, durability, excellent performance, simple preparation process, etc., and can be widely used in the fields of oil-water separation and emulsion demulsification. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0020] Figure 1 FTIR Fourier transform infrared spectra of the super hydrophobic activated carbon obtained in Example 1 and the super hydrophobic activated carbon obtained in Example 2 of the present invention;

[0021] Figure 2 This is a scanning electron microscope image of a 300-mesh super-hydrophobic activated carbon coating mesh prepared in Example 1 of the present invention, a is a low magnification, and b is a high magnification;

[0022] Figure 3 This is a scanning electron microscope image of a 2000-mesh super-hydrophobic activated carbon coating mesh prepared in Example 2 of the present invention, a is a low magnification, and b is a high magnification;

[0023] Figure 4 This is a water contact angle diagram of a 300-mesh super-hydrophobic activated carbon coating mesh prepared in Example 1 of the present invention;

[0024] Figure 5 This is the oil (chloroform) contact angle diagram of the 300-mesh super-hydrophobic activated carbon coating mesh prepared in Example 1 of the present invention;

[0025] Figure 6 This is a water contact angle diagram of a 2000-mesh super-hydrophobic activated carbon coating mesh prepared in Example 2 of the present invention;

[0026] Figure 7 This is the oil (chloroform) contact angle diagram of the 2000-mesh super-hydrophobic activated carbon coating mesh prepared in Example 2 of the present invention;

[0027] Figure 8The water contact angle change diagram of the 300-mesh super-hydrophobic activated carbon coating mesh prepared in Example 1 of the present invention during the durability test process, a is ultrasonic treatment, b is tape stripping, c is baking at different temperatures, and d is immersion in different pH solutions and seawater;

[0028] Fig. 9 It is a schematic diagram of the oil-water separation efficiency of the 300-mesh super-hydrophobic activated carbon coating mesh prepared in Example 1 of the present invention for five kinds of oil-water mixtures;

[0029] Fig.10 Schematic diagram of the efficiency and separation flux of the 300-mesh super-hydrophobic activated carbon coating net prepared in Example 1 of the present invention for separating a chloroform-water mixture for ten consecutive cycles;

[0030] Fig.11 Schematic diagram of the demulsification efficiency separation experiment of five water-in-oil emulsions using the 2000-mesh super-hydrophobic activated carbon coating mesh prepared in Example 2 of the present invention.

[0031] Fig.12 This is a water contact angle diagram of a 300-mesh super-hydrophobic activated carbon coating mesh prepared in Comparative Example 1 of the present invention;

[0032] Fig.13 This is the oil (chloroform) contact angle diagram of the 300-mesh super-hydrophobic activated carbon coating mesh prepared in Comparative Example 1 of the present invention;

[0033] Fig.14 This is a water contact angle diagram of a 300-mesh super-hydrophobic activated carbon coating mesh prepared in Comparative Example 2 of the present invention;

[0034] Fig.15 This is the oil (chloroform) contact angle diagram of the 300-mesh super-hydrophobic activated carbon coating mesh prepared in Comparative Example 2 of the present invention;

[0035] Fig.16 This is a water contact angle diagram of a 300-mesh super-hydrophobic activated carbon coating mesh prepared in Comparative Example 3 of the present invention;

[0036] Fig.17 This is the oil (chloroform) contact angle diagram of the 300-mesh super-hydrophobic activated carbon coating mesh prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0037] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0038] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0039] In view of the fact that the materials used in existing oil-water coatings are relatively expensive, and the present invention has found that relatively cheap activated carbon is difficult to use as a super-hydrophobic coating material after being super-hydrophobic modified using existing methods, the present invention proposes a super-hydrophobic activated carbon coating material and its preparation method and application.

[0040] A typical embodiment of the present invention provides a method for preparing a super-hydrophobic activated carbon coating material, comprising the following steps:

[0041] The activated carbon is washed until the hydroxyl groups on its surface are exposed;

[0042] The cleaned activated carbon is reacted with an organosilane in an alkaline system containing water, so that the organosilane is hydrolyzed and chemically bonded to the hydroxyl groups on the surface of the activated carbon, and the organosilane grafted on the surface of the activated carbon is polymerized to obtain a super-hydrophobic activated carbon; wherein the carbon number of the alkyl group of the organosilane is not less than 10;

[0043] The super-hydrophobic activated carbon and the resin binder are uniformly mixed in a solvent to obtain the super-hydrophobic activated carbon.

[0044] In some embodiments, the activated carbon is wood activated carbon, coconut shell activated carbon or coal-based activated carbon. Specifically, the particle size of the activated carbon is 200-500 mesh.

[0045] In some embodiments, washing the activated carbon with ethanol and water in sequence can better expose the hydroxyl groups on the surface of the activated carbon.

[0046] In certain embodiments, the activated carbon after cleaning is added to an alcohol solvent and is uniformly dispersed, then water is added, and the pH of the solvent system is alkalescent, and then an organosilane is added to react. First, the activated carbon is uniformly dispersed, and then an organosilane is added, which is conducive to fully contacting the surface of the activated carbon with the surface of the activated carbon, ensuring the grafting efficiency of the hydrophobic long carbon chain on the surface of the activated carbon, and improving the super-hydrophobic performance of the super-hydrophobic activated carbon. In order to make the activated carbon uniformly dispersed in an alcohol solvent, specifically, ultrasonic dispersion is adopted. The alcohol solvent of the present invention is a liquid alcohol organic matter, such as methanol, ethanol, propanol, ethylene glycol, etc., which is miscible with water, and is conducive to the reaction.

[0047] In some embodiments, the mass ratio of organosilane to activated carbon is (0.5-1.2):1.

[0048] The alkaline system described in the present invention is a reaction system with a pH greater than 7. In some embodiments, the pH value of the alkaline system is 9 to 11. The pH of the alkaline system can be adjusted using ammonia water, sodium hydroxide solution, etc.

[0049] In some embodiments, the mass ratio of added water to activated carbon is (1-2):1.

[0050] In some embodiments, the organosilane is one or a combination of dodecyltrichlorosilane, hexadecyltrichlorosilane, octadecyltrichlorosilane, dodecyltrimethoxysilane, hexadecyltrimethoxysilane, octadecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltriethoxysilane, and octadecyltriethoxysilane.

[0051] In some embodiments, the reaction time is 6 to 12 hours.

[0052] In some embodiments, the super-hydrophobic activated carbon is added to the alcohol solvent and dispersed evenly, and then the resin binder solution is added. Dispersing the super-hydrophobic activated carbon evenly first is conducive to mixing evenly with the resin binder, ensuring the stability of the super-hydrophobic property of the coating material.

[0053] In some embodiments, the resin binder is epoxy resin and its curing agent. Specifically, the epoxy resin model is E51, and the curing agent model is W93.

[0054] Another embodiment of the present invention provides a super hydrophobic activated carbon coating material obtained by the above preparation method.

[0055] A third embodiment of the present invention provides a super hydrophobic activated carbon coating, wherein the super hydrophobic activated carbon coating material is attached to the surface of a substrate.

[0056] In some embodiments, the attachment method is coating. The coating method includes spraying, dripping, dipping, etc. After coating, curing is performed. The curing temperature is 60 to 120° C. and the curing time is 4 to 8 hours.

[0057] In some embodiments, the substrate is one or more of stainless steel mesh, cotton cloth, polyurethane sponge, etc.

[0058] A fourth embodiment of the present invention provides an application of the above-mentioned super-hydrophobic activated carbon coating material or super-hydrophobic activated carbon coating in oil-water separation and / or emulsion demulsification.

[0059] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.

[0060] Example 1

[0061] (1) After the activated carbon is crushed, it is washed in anhydrous ethanol and deionized water in sequence until it is neutral, and then dried to obtain pretreated activated carbon.

[0062] (2) 5 g of pretreated activated carbon was added to 80 g of anhydrous ethanol for ultrasonic dispersion for 10 min, magnetic stirring was performed for 10 min, 10 g of water was added, and ammonia water was added to adjust the pH to 10 to obtain an activated carbon suspension.

[0063] (3) Add 5 g of hexadecyltrimethoxysilane to the activated carbon suspension, stir magnetically for 6 h, filter, and dry at 80 °C for 6 h to obtain super hydrophobic modified activated carbon, such as Figure 1 shown.

[0064] (4) 2 g of super-hydrophobic modified activated carbon was added to 50 g of anhydrous ethanol and ultrasonically dispersed for 10 min, and magnetically stirred for 10 min to obtain a super-hydrophobic modified activated carbon suspension.

[0065] (5) Add 1 g of E51 epoxy resin and 0.3 g of W93 curing agent to 4 g of anhydrous ethanol, ultrasonically disperse for 10 min and stir until the solution is clear and transparent to obtain an epoxy resin solution.

[0066] (6) Add the epoxy resin solution to the super-hydrophobic modified activated carbon suspension and stir for 30 minutes to obtain a super-hydrophobic activated carbon coating solution.

[0067] (7) The super-hydrophobic activated carbon coating solution was added to a spray gun and sprayed on the surface of a 300-mesh stainless steel mesh. The distance between the spray gun and the substrate was 15 cm, the spraying pressure was 0.5 MPa, the moving speed was 3 cm / s, and the curing temperature was 80 ° C for 6 h to obtain a 300-mesh super-hydrophobic activated carbon coating mesh. Figure 2 shown.

[0068] The 300-mesh super-hydrophobic activated carbon coating mesh of this embodiment was subjected to wettability testing, durability testing, and oil-water separation efficiency testing.

[0069] The water contact angle of the 300-mesh superhydrophobic activated carbon coated mesh is 155.1°. Figure 4 shown.

[0070] The oil contact angle of the 300-mesh superhydrophobic activated carbon coated mesh is about 0°, e.g. Figure 5 shown.

[0071] The water sliding angle of the 300-mesh superhydrophobic activated carbon coated mesh is 8.9°.

[0072] The durability test of the 300-mesh super-hydrophobic activated carbon coating net showed that after 120W ultrasound for 300 minutes, tape stripping for 20 times, baking at 200℃ for 1 hour, and soaking in various pH solutions and seawater for 24 hours, the 300-mesh super-hydrophobic activated carbon coating net still maintained its super-hydrophobicity. Figure 8 shown.

[0073] Five kinds of oil-water mixtures (chloroform-water, chlorobenzene-water, n-hexane-water, gasoline-water, sweet almond oil-water) were separated using a 300-mesh super-hydrophobic activated carbon coated net. By measuring the water content in the oil-water mixtures before and after separation, it was found that the oil-water separation efficiency of the 300-mesh super-hydrophobic activated carbon coated net for the five oil-water mixtures was 98.6%, 99.2%, 99.4%, 96.7%, and 96.5%, respectively. Fig. 9 shown.

[0074] The efficiency and separation flux of 300-mesh superhydrophobic activated carbon coated mesh in separating chloroform-water mixture for ten consecutive cycles were tested. The efficiency of each of the ten cycles of separating chloroform-water mixture was above 95%, and the separation flux was maintained at 12000 L·m -2 ·h -1 ,like Fig.10 shown.

[0075] Example 2

[0076] (1) After the activated carbon is crushed, it is washed in anhydrous ethanol and deionized water in sequence until it is neutral, and then dried to obtain pretreated activated carbon.

[0077] (2) 10 g of pretreated activated carbon was added to 200 g of anhydrous ethanol, ultrasonically dispersed for 10 min, magnetically stirred for 10 min, 20 g of water was added, and ammonia water was added to adjust the pH to 11 to obtain an activated carbon suspension.

[0078] (3) Add 20 g of dodecyltriethoxysilane to the activated carbon suspension, stir magnetically for 12 h, filter, and dry at 60 °C for 12 h to obtain super hydrophobic modified activated carbon, such as Figure 1 shown.

[0079] (4) Add 5 g of super-hydrophobic modified activated carbon into 50 g of anhydrous ethanol and disperse it ultrasonically for 10 min. Then, stir it magnetically for 10 min to obtain a super-hydrophobic modified activated carbon suspension.

[0080] (5) Add 2 g of E51 epoxy resin and 0.5 g of W93 curing agent to 10 g of anhydrous ethanol, ultrasonically disperse for 10 min and stir evenly until the solution is clear and transparent to obtain an epoxy resin solution.

[0081] (6) Add the epoxy resin solution to the super-hydrophobic modified activated carbon suspension and stir for 30 minutes to obtain a super-hydrophobic activated carbon coating solution.

[0082] (7) The super-hydrophobic activated carbon coating solution was added to the spray gun and sprayed on the surface of the 2000 mesh stainless steel mesh. The distance between the spray gun and the substrate was 15 cm, the spraying pressure was 0.5 MPa, the moving speed was 3 cm / s, and the curing temperature was 60 ° C for 8 h to obtain a 2000 mesh super-hydrophobic activated carbon coating mesh. Figure 3 shown.

[0083] The 2000-mesh super-hydrophobic activated carbon coating mesh of this embodiment was subjected to wettability testing and oil-water separation efficiency testing.

[0084] The water contact angle of the 2000 mesh super-hydrophobic activated carbon coated mesh is 154.5°. Figure 6 shown.

[0085] The oil contact angle of the 2000 mesh super-hydrophobic activated carbon coated mesh is about 0°, e.g. Figure 7 shown.

[0086] The water sliding angle of the 2000-mesh superhydrophobic activated carbon coated mesh is 9.3°.

[0087] Five kinds of oil-in-water emulsions (chloroform-water, chlorobenzene-water, n-hexane-water, gasoline-water) were demulsified using a 2000-mesh super-hydrophobic activated carbon coated mesh. By measuring the water content in the oil-in-water emulsions before and after separation, it was found that the demulsification efficiencies of the 2000-mesh super-hydrophobic activated carbon coated mesh for the five kinds of oil-in-water emulsions were 93.8%, 96.7%, 96.1%, and 94.2%, respectively. Fig.11 shown.

[0088] Comparative Example 1

[0089] (1) After the activated carbon is crushed, it is washed in anhydrous ethanol and deionized water in sequence until it is neutral, and then dried to obtain pretreated activated carbon.

[0090] (2) Add 5 g of pretreated activated carbon to 80 g of anhydrous ethanol and disperse it ultrasonically for 10 min. Then stir it magnetically for 10 min to obtain an activated carbon suspension.

[0091] (3) Add 5 g of hexadecyltrimethoxysilane to the activated carbon suspension, heat to reflux, magnetically stir for 6 h, filter, and dry at 80 °C for 6 h to obtain super hydrophobic modified activated carbon.

[0092] (4) 2 g of super-hydrophobic modified activated carbon was added to 50 g of anhydrous ethanol and ultrasonically dispersed for 10 min, and magnetically stirred for 10 min to obtain a super-hydrophobic modified activated carbon suspension.

[0093] (5) Add 1 g of E51 epoxy resin and 0.3 g of W93 curing agent to 4 g of anhydrous ethanol, ultrasonically disperse for 10 min and stir until the solution is clear and transparent to obtain an epoxy resin solution.

[0094] (6) Add the epoxy resin solution to the super-hydrophobic modified activated carbon suspension and stir for 30 minutes to obtain a super-hydrophobic activated carbon coating solution.

[0095] (7) The super-hydrophobic activated carbon coating solution was added to the spray gun and sprayed on the surface of a 300-mesh stainless steel mesh. The distance between the spray gun and the substrate was 15 cm, the spraying pressure was 0.5 MPa, the moving speed was 3 cm / s, and the curing temperature was 80 ° C for 6 h to obtain a 300-mesh super-hydrophobic activated carbon coating mesh.

[0096] The wettability test was performed on the 300-mesh super-hydrophobic activated carbon coating mesh of this comparative example.

[0097] The water contact angle of the 300-mesh superhydrophobic activated carbon coated mesh is 135.6°. Fig.12 shown.

[0098] The oil contact angle of the 300-mesh superhydrophobic activated carbon coated mesh is about 0°, e.g. Fig.13 shown.

[0099] The water sliding angle of the 300-mesh superhydrophobic activated carbon coated mesh is 27.2°.

[0100] Comparative Example 1 Compared with Example 1, when preparing super-hydrophobic activated carbon, Comparative Example 1 does not add water or adjust pH to alkalinity, and the 300-mesh super-hydrophobic activated carbon coating net prepared by it does not have super-hydrophobic performance. The main reason is that without adding water or adjusting pH to alkalinity, organosilane cannot be hydrolyzed and polymerized, and can only be super-hydrophobic modified by surface physical adsorption of the pore structure of activated carbon, but in the subsequent process of adding anhydrous ethanol, the organosilane adsorbed on the surface of activated carbon will be desorbed due to anhydrous ethanol washing, so that the 300-mesh super-hydrophobic activated carbon coating net made is far from the requirement of super-hydrophobic performance.

[0101] Comparative Example 2

[0102] (1) After the activated carbon is crushed, it is washed in anhydrous ethanol and deionized water in sequence until it is neutral, and then dried to obtain pretreated activated carbon.

[0103] (2) Add 5 g of pretreated activated carbon to 80 g of anhydrous ethanol and disperse it ultrasonically for 10 min. Then, stir it magnetically for 10 min and add 10 g of water to obtain an activated carbon suspension.

[0104] (3) Add 5 g of hexadecyltrimethoxysilane to the activated carbon suspension, heat to reflux, magnetically stir for 6 h, filter, and dry at 80 °C for 6 h to obtain super hydrophobic modified activated carbon.

[0105] (4) 2 g of super-hydrophobic modified activated carbon was added to 50 g of anhydrous ethanol and ultrasonically dispersed for 10 min, and magnetically stirred for 10 min to obtain a super-hydrophobic modified activated carbon suspension.

[0106] (5) Add 1 g of E51 epoxy resin and 0.3 g of W93 curing agent to 4 g of anhydrous ethanol, ultrasonically disperse for 10 min and stir until the solution is clear and transparent to obtain an epoxy resin solution.

[0107] (6) Add the epoxy resin solution to the super-hydrophobic modified activated carbon suspension and stir for 30 minutes to obtain a super-hydrophobic activated carbon coating solution.

[0108] (7) The super-hydrophobic activated carbon coating solution was added to the spray gun and sprayed on the surface of a 300-mesh stainless steel mesh. The distance between the spray gun and the substrate was 15 cm, the spraying pressure was 0.5 MPa, the moving speed was 3 cm / s, and the curing temperature was 80 ° C for 6 h to obtain a 300-mesh super-hydrophobic activated carbon coating mesh.

[0109] The wettability test was performed on the 300-mesh super-hydrophobic activated carbon coating mesh of this comparative example.

[0110] The water contact angle of the 300-mesh superhydrophobic activated carbon coated mesh is 149.3°. Fig.14 shown.

[0111] The oil contact angle of the 300-mesh superhydrophobic activated carbon coated mesh is about 0°, e.g. Fig.15 shown.

[0112] The water sliding angle of the 300-mesh superhydrophobic activated carbon coated mesh is 13.7°.

[0113] Comparative Example 2 is compared with Comparative Example 1 and Example 1, and when preparing super-hydrophobic activated carbon, Comparative Example 2 does not adjust pH to alkalinity, and 300 mesh super-hydrophobic activated carbon coating nets hydrophobicity prepared by it is higher than Comparative Example 1, close to super-hydrophobicity, but fails to reach super-hydrophobicity (water contact is less than 150 °). pH is not adjusted to alkalinity, and the silanol of organosilane hydrolysis can not be further polymerized, so that it is impossible to ensure that the hydrophobic long carbon chain is firmly fixed on the activated carbon surface, so that the coating material prepared later cannot reach the requirement of super-hydrophobicity.

[0114] Comparative Example 3

[0115] (1) The activated carbon is crushed and dried to obtain pretreated activated carbon.

[0116] (2) 5 g of pretreated activated carbon was added to 80 g of anhydrous ethanol for ultrasonic dispersion for 10 min, magnetic stirring was performed for 10 min, 10 g of water was added, and ammonia water was added to adjust the pH to 10 to obtain an activated carbon suspension.

[0117] (3) Add 5 g of hexadecyltrimethoxysilane to the activated carbon suspension, heat to reflux, magnetically stir for 6 h, filter, and dry at 80 °C for 6 h to obtain super hydrophobic modified activated carbon.

[0118] (4) 2 g of super-hydrophobic modified activated carbon was added to 50 g of anhydrous ethanol and ultrasonically dispersed for 10 min, and magnetically stirred for 10 min to obtain a super-hydrophobic modified activated carbon suspension.

[0119] (5) Add 1 g of E51 epoxy resin and 0.3 g of W93 curing agent to 4 g of anhydrous ethanol, ultrasonically disperse for 10 min and stir until the solution is clear and transparent to obtain an epoxy resin solution.

[0120] (6) Add the epoxy resin solution to the super-hydrophobic modified activated carbon suspension and stir for 30 minutes to obtain a super-hydrophobic activated carbon coating solution.

[0121] (7) The super-hydrophobic activated carbon coating solution was added to the spray gun and sprayed on the surface of a 300-mesh stainless steel mesh. The distance between the spray gun and the substrate was 15 cm, the spraying pressure was 0.5 MPa, the moving speed was 3 cm / s, and the curing temperature was 80 ° C for 6 h to obtain a 300-mesh super-hydrophobic activated carbon coating mesh.

[0122] The wettability test was performed on the 300-mesh super-hydrophobic activated carbon coating mesh of this comparative example.

[0123] The water contact angle of the 300-mesh superhydrophobic activated carbon coated mesh is 146.5°. Fig.16 shown.

[0124] The oil contact angle of the 300-mesh superhydrophobic activated carbon coated mesh is about 0°, e.g. Fig.17 shown.

[0125] The water sliding angle of the 300-mesh superhydrophobic activated carbon coated mesh is 17.1°.

[0126] Compared with Example 1, the activated carbon was not cleaned, and the hydrophobicity of the 300-mesh super-hydrophobic activated carbon coating net prepared therefrom failed to reach the super-hydrophobic performance (water contact is less than 150°). The main reason is that the activated carbon was not cleaned, resulting in incomplete exposure of the surface hydroxyl groups, which led to incomplete grafting of the subsequent super-hydrophobic modification, and thus failed to meet the requirements of super-hydrophobic performance.

[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a super-hydrophobic activated carbon coating material, comprising: The process is as follows: The activated carbon is washed until the hydroxyl groups on its surface are exposed; The cleaned activated carbon is reacted with an organosilane in an alkaline system containing water, so that the organosilane is hydrolyzed and chemically bonded to the hydroxyl groups on the surface of the activated carbon, and the organosilane grafted on the surface of the activated carbon is polymerized to obtain a super-hydrophobic activated carbon; wherein the carbon number of the alkyl group of the organosilane is not less than 10; The super-hydrophobic activated carbon and the resin binder are uniformly mixed in a solvent to obtain the super-hydrophobic activated carbon.

2. The method for preparing a super hydrophobic activated carbon coating material according to claim 1, wherein: The activated carbon was washed with ethanol and water in sequence.

3. The method for preparing a super hydrophobic activated carbon coating material according to claim 1, wherein: The cleaned activated carbon is added to an alcohol solvent and dispersed evenly, water is added, and the pH of the solvent system is adjusted to be alkaline, and then organic silane is added to react.

4. The method for preparing a super hydrophobic activated carbon coating material according to claim 1, wherein: The mass ratio of organosilane to activated carbon is (0.5-1.2):1; Or, the pH value of the alkaline system is 9 to 11; Or, the mass ratio of added water to activated carbon is (1-2):1; Or, the reaction time is 6 to 12 hours.

5. The method for preparing a super hydrophobic activated carbon coating material according to claim 1, wherein: The super-hydrophobic activated carbon is added to the alcohol solvent and dispersed evenly, and then the resin binder solution is added.

6. The method for preparing a super hydrophobic activated carbon coating material according to claim 1, wherein: The resin binder is epoxy resin and its curing agent.

7. A super hydrophobic activated carbon coating material, characterized in that: Obtained by the preparation method according to any one of claims 1 to 6.

8. A super hydrophobic activated carbon coating, characterized in that: The super-hydrophobic activated carbon coating material according to claim 7 is attached to the surface of the substrate.

9. The super hydrophobic activated carbon coating according to claim 8, characterized in that: The method of attachment is coating; Or, the substrate is one or more of stainless steel mesh, cotton cloth, and polyurethane sponge.

10. Application of the above-mentioned super-hydrophobic activated carbon coating material or super-hydrophobic activated carbon coating in oil-water separation and / or emulsion demulsification.

Citation Information

Patent Citations

  • Preparation method of hydrophobic activated carbon modified material

    CN104437444A

  • Superhydrophobic powder coating and preparation method thereof

    CN109651920A

  • Oil-water separation structure with super-hydrophobic / super-oleophylic performance as well as preparation method and application of oil-water separation structure

    CN111437627A

  • Preparation method of activated carbon material surface hydrophobic protective layer

    CN111589414A

  • Super-hydrophobic oleophylic polyurethane sponge and preparation method thereof

    CN115160640A

Cited By

  • Super-hydrophobic activated carbon adsorption material as well as preparation method and application thereof

    CN119819263A

  • Super-hydrophobic activated carbon adsorption material, and preparation method and application thereof

    CN119819263B