Foam metal catalyst and application thereof in nitro hydrogenation

By loading the active metal onto the foam nickel copper and applying it in the micro reactor, the problems of poor dispersion and mass transfer resistance in the traditional catalyst preparation method are solved, and efficient nitro hydrogenation reaction is achieved, and catalytic performance is improved. and stability, suitable for a variety of nitro substance conditions.

CN119076014APending Publication Date: 2024-12-06浙江友联化学工业有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411208882.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The traditional catalyst preparation method has problems such as poor dispersion of the catalyst and large mass transfer resistance, which affects the efficiency and selectivity of the reaction. In the prior art, there are problems such as loss of active metals and inapplicable selective hydrogenation in the nitro hydrogenation reaction. .

Method used

By loading the active metal onto the foam nickel-copper foam, a metal-supported foam nickel-copper catalyst is prepared and applied in a micro reactor. The metal loading and pore structure are controlled by using steps such as hydrothermal treatment and calcination, and combined with an appropriate amount of inhibitor to prevent dehalogenation. , improve the stability and reaction performance of the catalyst.

Benefits of technology

It significantly improves the catalytic performance and reaction rate, improves temperature control and thermal equilibrium capabilities, and is suitable for a variety of nitro substances, including halogen-free and halogen-free conditions, enhancing the stability and selectivity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076014A_ABST
    Figure CN119076014A_ABST
Patent Text Reader

Abstract

The invention provides a foam metal catalyst and application thereof in nitro hydrogenation, and relates to the technical field of catalytic hydrogenation. The foam metal catalyst is a metal-loaded foam nickel-copper catalyst, and the metal-loaded foam nickel-copper catalyst is filled in the microreactor for nitro hydrogenation reaction; the metal-loaded foamed nickel-copper catalyst is obtained by pretreating foamed nickel-copper in manners of cutting, cleaning, drying, pickling and the like, dipping in a metal solution to adsorb and load metal active components, and roasting. The defects in the prior art are overcome, the efficient heat transfer and mass transfer characteristics of the microreactor can be fully utilized, and meanwhile, the loading area of the catalyst is increased through the foam metal carrier, so that double advantages are brought, and the catalytic performance of the reactor is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalytic hydrogenation, and in particular to a foamed metal catalyst and application thereof in nitro hydrogenation. Background Art

[0002] Microchannel reactor is an efficient chemical reaction device with significant advantages in small size, large surface area ratio, heat transfer performance and operational safety. Traditional catalyst preparation methods often have problems such as poor catalyst dispersion and large mass transfer resistance, which affect the efficiency and selectivity of the reaction. Metal foam is composed of mesh pores and has a polyhedral shape. It has the characteristics of high specific surface area, low density, and large pore size. It is considered to be an ideal carrier material. Therefore, using metal foam as a catalyst carrier and loading active metals on its surface can effectively solve the problems of the above-mentioned traditional catalysts. Among them, copper-nickel foam (CNF) has a uniform pore structure and a large surface area, which can provide more active sites and enhance the contact between the catalyst and the reactant. At the same time, due to its good thermal conductivity, higher reaction rates and better temperature control can be achieved.

[0003] In order to ensure the long-term availability and sustainable use of catalyst materials, it is necessary to design high-temperature catalysts. Jurca et al. (Catal. Sci. Technol., 2022, 12, 6992) used a polydopamine (PDA) seed layer to grow a solid Pd nanocatalyst-coated foam Ni, which showed excellent catalytic activity for the hydrogenation of functionalized nitrobenzene and styrene at low temperature and low hydrogen pressure, and the catalyst was proven to be stable and easy to recover. However, this method may have the problem of active metal loss on the catalyst and is not suitable for selective hydrogenation. Once the halogenated aromatics are dehalogenated, they will corrode the foam Ni catalyst and the reactor. The hydrodynamic properties of gas-liquid two-phase flow will significantly affect the performance of the gas-liquid-solid microreactor. Zhu et al. (React. Chem. Eng., 2019, 4, 715-723) used visualization technology to study the flow behavior of multiphase catalytic reactions with nitrobenzene hydrogenation as a reference. In the reaction and non-reaction conditions, significant differences in the length evolution, migration velocity and residence time of the gas clusters were detected. The interface retraction of the gas mass was observed, which was mainly attributed to the hydrogen consumption during the pressure accumulation stage. The results of the microreactor hydrogenation performance showed that increasing the gas flow rate can improve the conversion of nitrobenzene, but the reduction of residence time at high gas flow rate weakened this effect. The method has the interface retraction of the gas mass and the backward velocity in the downstream increases, which is not conducive to the steady-state operation of multiphase flow. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a foam metal catalyst and its application in nitro hydrogenation, and realizes efficient hydrogenation reaction by loading active metals onto foam nickel copper.

[0005] To achieve the above objectives, the technical solution of the present invention is implemented through the following technical solutions:

[0006] A foamed metal catalyst, wherein the foamed metal catalyst is a metal-loaded nickel-copper foamed catalyst, and the metal-loaded nickel-copper foamed catalyst is loaded inside a microreactor, and the preparation method of the metal-loaded nickel-copper foamed catalyst comprises the following steps:

[0007] S1, cutting the nickel copper foam into a cylinder with the same inner diameter as the microreactor, and then fine grinding the cut surface with sandpaper, using an organic solvent to ultrasonically clean the surface impurities, and then drying and pickling, and finally washing with deionized water until neutral and drying;

[0008] S2. Prepare a metal solution, adjust the solution pH to 5-6, load the metal active components of the metal solution onto the pretreated nickel copper foam by hydrothermal treatment, then wash and dry, and calcine the nickel copper foam loaded with the metal active components under N2 atmosphere to obtain a foam metal catalyst; and control the loading amount of the metal active components to be 0.1-2.5wt% of the nickel copper foam.

[0009] Preferably, the copper content of the nickel copper foam in step S1 is 1% to 5%, the number of pores is 85 to 130 ppi, and the surface density is 200-600 g / m 2 .

[0010] Preferably, in step S1, the method of using an organic solvent to ultrasonically clean surface impurities is: selecting any one of ethanol and acetone as the organic solvent for ultrasonic cleaning for 5-10 minutes; the method of pickling is: selecting any one of hydrochloric acid, nitric acid and sulfuric acid as the pickling component, and controlling the acid concentration to 1-5 vol% and the pickling time to 2-10 minutes.

[0011] Preferably, the metal active component in step S2 is any one or more of Pt, Pd, Rh, Ru, and Co.

[0012] Preferably, the hydrothermal treatment in step S2 is performed by placing the nickel copper foam into a polytetrafluoroethylene liner containing a metal solution at a solid-liquid ratio of 1:10-20, heating the mixture to 80-160°C for a hydrothermal reaction for 2-12 hours; and the calcination treatment in step S2 is performed at 300-500°C for 1-3 hours.

[0013] The metal solution in step S2 can be recycled after impregnation, that is, the metal content and metal ion state in the metal solution after impregnation are respectively determined by atomic absorption spectrometer and ion chromatography; if it is detected that the impregnation solution contains copper and nickel, the impregnation solution is circulated through the ion exchange resin packed bed to accurately adsorb the divalent ions (Ni 2+ , Cu 2+ ) until the copper-nickel ion content is less than 0.02 mg / L; after the treatment is completed, the corresponding precious metal solution is added again to a certain concentration for the next round of impregnation.

[0014] Preferably, the mesh number of the ion exchange resin is 10 to 50, and the filling height is 20 to 60 cm.

[0015] Preferably, the flow rate of the impregnation liquid is 0.1-1 BV / h.

[0016] The foamed metal catalyst is used in a microreactor to carry out a nitro hydrogenation reaction. The applicable nitro substances include halogen-free nitrobenzene, halogenated nitrobenzene with a solvent, and halogenated nitrobenzene without a solvent. The specific operation steps include the following steps:

[0017] (1) Connecting a microreactor loaded with a foamed metal catalyst to a metal aeration head as a gas-liquid mixer;

[0018] (2) Under normal pressure, nitrogen is introduced to replace the air in the reaction tube, and then hydrogen is introduced. After the gas flow stabilizes, the catalyst is reduced;

[0019] (3) After the reduction is completed, turn off the nitrogen and adjust the hydrogen flow rate at the same time, wait for the temperature to drop to the reaction temperature, and then introduce the raw material liquid to start the reaction.

[0020] Preferably, in step (1), the inner diameter of the microreactor is 2-5 mm, and the bed height is 50-80 mm.

[0021] Preferably, the reduction temperature in step (2) is 250-400°C, and the reduction time is 2-4h; and the reaction temperature in step (3) is in the range of 70-150°C, the gas-liquid ratio is 20-50:1, and the liquid space velocity is 1-5h -1 .

[0022] Preferably, in step (3), when the raw material liquid is a solvent-containing halogenated nitrobenzene, an inhibitor is added to the raw material liquid at a mass ratio of 1-20:1, and the inhibitor is any one of ammonia water, ammonium bicarbonate, dicyandiamide, ethanolamine, and triethylamine.

[0023] The present invention provides a foam metal catalyst and its application in nitro hydrogenation, which has the following advantages over the prior art:

[0024] (1) The present invention applies a foamed metal catalyst to a microreactor, which can make full use of the efficient heat and mass transfer characteristics of the microreactor, and at the same time increase the catalyst loading area through the foamed metal carrier, thereby bringing a double advantage to significantly improve the catalytic performance of the reactor. Since the foamed metal has a small flow resistance to the fluid, the gas-liquid-solid three-phase mass transfer performance can be greatly improved, and the foamed metal catalyst has excellent thermal conductivity and a large interfacial area at the microscale, which can achieve rapid and uniform heat transfer, and improve the temperature control and thermal balance capabilities of the reactor.

[0025] (2) The foamed metal catalyst of the present invention has a uniform pore structure, which can promote the mass transfer of reactants and quickly diffuse to the catalyst surface during the reaction, thereby reducing the internal mass transfer resistance and increasing the reaction rate.

[0026] (3) The present invention can be applied to most nitro compounds (including halogenated and halogen-free compounds), and is also applicable to conditions with or without solvents. For the hydrogenation reaction of halogenated nitrobenzene in the presence of solvents, dehalogenation can be effectively prevented by adding an appropriate amount of inhibitor, thereby improving the stability of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the microreactor structure used in the embodiment of the present invention;

[0028] Among them: 1-air inlet, 2-liquid storage tank, 3-micro peristaltic pump, 4-liquid inlet, 5-microchannel reactor, 6-gas-liquid distributor, 7-foam metal catalyst, 8-discharge port. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Set as Figure 1 The microchannel reactor 5 shown in the figure has a gas-liquid distributor 6 arranged at the upper end of the microchannel reactor 5 which is connected to the gas inlet 1 and the liquid inlet 4, and the liquid inlet 4 is connected to the liquid storage tank 2 through a micro peristaltic pump 3, the inside of the microchannel reactor 5 is filled with a foamed metal catalyst 7, and the lower end of the microchannel reactor 5 is a discharge port 8.

[0031] Example:

[0032] Preparation of metal-supported nickel-copper foam catalyst:

[0033] The copper content is 1%, the number of holes is 85ppi, and the surface density is 200g / m 2 The nickel copper foam was cut into a cylinder with the same inner diameter as the microreactor, with a diameter of 2.5 mm and a height of 60 mm, and the cut surface was finely ground with sandpaper; then, it was ultrasonically cleaned with ethanol for 10 minutes; after cleaning, it was cleaned with 3 vol% hydrochloric acid for 5 minutes; finally, it was washed with deionized water until it was neutral and dried;

[0034] Prepare a metal solution: wherein the metal active component is Pt, and use a 1M concentration NaOH solution to adjust the pH value of the metal solution to 5.2; place the pretreated nickel copper foam into a polytetrafluoroethylene liner containing the above-mentioned Pt solution at a solid-liquid ratio of 1:10, and perform hydrothermal treatment at a temperature of 100°C for 6 hours; after the hydrothermal treatment, wash with deionized water and dry; and perform calcination treatment under a N2 atmosphere at a temperature of 400°C for 2 hours to obtain a Pt / NCF catalyst with a Pt loading of 0.3wt%.

[0035] For the metal solution after the impregnation, the metal content and metal ion state in the solution are detected by atomic absorption spectrometer and ion chromatography; when copper and nickel ions are detected in the solution, the impregnation solution is circulated through an ion exchange resin packed bed, the mesh number of the resin is 20-30, the filling height is 40cm, and the flow rate of the impregnation solution is 0.5BV / h, until the copper and nickel ion content in the impregnation solution is less than or equal to 0.02mg / L. Then the corresponding precious metal solution is added to a certain concentration for the next round of impregnation.

[0036] In such Figure 1 The prepared 0.3wt% Pt / NCF catalyst is loaded into the microreactor 5, and a metal aeration head is connected as a gas-liquid mixer 6. After the reactor is installed, nitrogen is used to replace the air in the reaction tube under normal pressure. Then hydrogen is introduced and the flow rate is adjusted to be stable. After the airflow stabilizes, the catalyst is reduced. The reduction temperature is 250°C and the reduction time is 2h. When the reduction is completed, the nitrogen is turned off and the hydrogen flow rate is adjusted at the same time to reduce the temperature to the reaction temperature. The reaction temperature is set to 70°C, the gas-liquid ratio is 20, and the liquid space velocity is 2h -1 A halogenated nitrobenzene raw material solution containing an inhibitor was introduced, wherein the concentration of p-chloronitrobenzene was 0.05 g / mL, the solvent was methanol, and the molar ratio of the inhibitor ammonia water to p-chloronitrobenzene was 1:10.

[0037] Referring to the above operation, different parameters were adjusted to design different experimental groups and control groups. The specific parameter adjustments are shown in Table 1 below:

[0038] Table 1

[0039]

[0040]

[0041] The application conditions and parameters of the above experimental groups and control groups in the specific nitro hydrogenation reaction are shown in Table 2 below:

[0042] Table 2

[0043]

[0044]

[0045] The conversion rate and selectivity of the nitro hydrogenation reaction of the above experimental group and the control group were tested, and the specific results are shown in Table 3 below:

[0046] Table 3

[0047]

[0048] It can be seen from the above table that the methods of experimental groups 1-10 can effectively ensure the conversion rate and selectivity of the nitro hydrogenation reaction.

[0049] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A foamed metal catalyst, characterized in that: The foam metal catalyst is a metal-loaded nickel-copper foam catalyst, and the metal-loaded nickel-copper foam catalyst is loaded inside a microreactor. The preparation method of the metal-loaded nickel-copper foam catalyst comprises the following steps: S1, cutting the nickel copper foam into a cylinder with the same inner diameter as the microreactor, and then fine grinding the cut surface with sandpaper, using an organic solvent to ultrasonically clean the surface impurities, and then drying and pickling, and finally washing with deionized water until neutral and drying; S2. Prepare a metal solution, adjust the solution pH to 5-6, load the metal active components of the metal solution onto the pretreated nickel copper foam by hydrothermal treatment, then wash and dry, and calcine the nickel copper foam loaded with the metal active components under N2 atmosphere to obtain a foam metal catalyst; and control the loading amount of the metal active components to be 0.1-2.5wt% of the nickel copper foam.

2. The foamed metal catalyst according to claim 1, characterized in that: The copper content of the nickel copper foam in step S1 is 1% to 5%, the number of pores is 85 to 130 ppi, and the surface density is 200-600 g / m 2 .

3. The foamed metal catalyst according to claim 1, characterized in that In step S1, the method of using an organic solvent to ultrasonically clean surface impurities is: selecting any one of ethanol and acetone as the organic solvent for ultrasonic cleaning for 5-10 minutes; the method of pickling is: selecting any one of hydrochloric acid, nitric acid and sulfuric acid as the pickling component, and controlling the acid concentration to be 1-5 vol% and the pickling time to be 2-10 minutes.

4. The foamed metal catalyst according to claim 1, characterized in that: The metal active component in step S2 is any one or more of Pt, Pd, Rh, Ru, and Co.

5. The foamed metal catalyst according to claim 1, characterized in that: The hydrothermal treatment method in step S2 is to place the foamed nickel copper into a polytetrafluoroethylene liner containing a metal solution at a solid-liquid ratio of 1:10-20, and heat it to 80-160°C for hydrothermal reaction for 2-12 hours; and the calcination treatment method in step S2 is to calcine at a temperature of 300-500°C for 1-3 hours.

6. Use of the foamed metal catalyst according to any one of claims 1 to 5 in catalytic nitro hydrogenation reactions.

7. The use according to claim 6, characterized in that: The nitro compounds applicable to the nitro hydrogenation reaction include halogen-free nitrobenzene, halogenated nitrobenzene with solvent, and halogenated nitrobenzene without solvent, and the specific operation steps include the following steps: (1) Connecting a microreactor loaded with a foamed metal catalyst to a metal aeration head as a gas-liquid mixer; (2) Under normal pressure, nitrogen is introduced to replace the air in the reaction tube, and then hydrogen is introduced. After the gas flow stabilizes, the catalyst is reduced; (3) After the reduction is completed, turn off the nitrogen and adjust the hydrogen flow rate at the same time, wait for the temperature to drop to the reaction temperature, and then introduce the raw material liquid to start the reaction.

8. The application according to claim 7, characterized in that: In the step (1), the inner diameter of the microreactor is 2-5 mm, and the bed height is 50-80 mm.

9. The use according to claim 7, characterized in that: The reduction temperature in step (2) is 250-400°C, and the reduction time is 2-4h; and the reaction temperature in step (3) is in the range of 70-150°C, the gas-liquid ratio is 20-50:1, and the liquid space velocity is 1-5h -1 .

10. The use according to claim 7, characterized in that: In the step (3), when the raw material liquid is halogenated nitrobenzene with a solvent, an inhibitor is added to the raw material liquid at a mass ratio of 1-20:1, and the inhibitor is any one of ammonia water, ammonium bicarbonate, dicyandiamide, ethanolamine, and triethylamine.