Manufacturing method of iron-nickel base alloy large-diameter thin-wall seamless tube
Through the secondary heat perforation forming method, the thermal perforation pass deformation amount and rolling parameters are adjusted, and the problem of difficult production of large-diameter thin-walled pipes of iron-nickel-based alloys in the prior art is solved, and the production of diameter-wall ratio >13 is achieved, reducing the reduction of The cold processing pass and energy consumption are improved, and the yield rate is improved.
Patent Information
- Application Number
- CN202411272889.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-06
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of production of seamless iron-nickel alloy steel pipes, and in particular to a method for manufacturing large-diameter, thin-walled seamless iron-nickel alloy pipes. Background Art
[0002] Iron-nickel-based alloy is an alloy material with excellent high-temperature performance, mainly composed of nickel, iron, chromium and other elements. Its advantages are high corrosion resistance, high-temperature strength and good machinability. The strength and corrosion resistance at high temperature are very excellent, and it can withstand corrosion from various corrosive media such as acids, alkalis, and salts. It is mainly used in heat exchangers, various reactors, furnace tubes, catalysts and other components of equipment such as oil refining, chemical industry, and synthetic ammonia. At present, the production of seamless steel pipes of iron-nickel-based alloys is generally produced by hot rolling perforation or hot extrusion + cold expansion / rolling process. Hot rolling perforation has good economic efficiency, but the deformation amount is small due to the influence of material properties during the perforation process, and only thick-walled pipes with a diameter-to-wall ratio of ≤10 can be produced, resulting in a series of problems such as an increase in subsequent cold expansion / rolling passes, repeated heat treatment, an increase in process passes, and increased energy consumption; although hot extrusion can produce products with a large diameter-to-wall ratio, the overall yield rate is only about 85% of perforation.
[0003] The present invention adopts a secondary hot perforation forming method to successfully produce a large-diameter thin-walled seamless nickel-based alloy tube with a diameter-to-wall ratio greater than 13, thereby reducing the number of subsequent cold processing passes, improving the yield rate, and solving a series of problems. Summary of the invention
[0004] The purpose of the present invention is to provide a method for manufacturing a large-diameter, thin-walled seamless iron-nickel alloy pipe in view of the above problems.
[0005] The object of the present invention is achieved in this way: a method for manufacturing a large-diameter thin-walled seamless iron-nickel alloy pipe comprises the following steps: step 1: blank requirements: the blank is subjected to electroslag remelting + radial forging + lathing + ultrasonic inspection, and the blank chemical composition requirements are: C: 0.06-0.1%, Si≤1%, Mn: 1.0-1.5%, P≤0.01%, S≤0.01%, Cr: 19-23%, Ni: 30-35%, Cu: 0.5-0.75%, Fe: 39.5-47%, Al: 0.15-0.6%, Ti: 0.15-0.6%; size requirements: φ200mm-300mm blank Material, outer diameter tolerance -1.8 / +0mm; Ultrasonic inspection: For billets of φ200mm-300mm, the maximum flat-bottom hole diameter corresponding to the flaw detection sensitivity is φ3mm; Step 2: Billet processing: Billet peeling: Peel the billet, the peeling amount is 1.5-2mm on one side, and the surface roughness after peeling is Ra<4μm; Billet sawing: Cut the billet by sawing, and the deviation of the vertical line between the section and the billet axis after sawing is ≤3mm; Billet centering: Punch a hole at the center of the billet, and the punching diameter is 20-80mm; Step 3: Pipe heating: Place the billet in an inclined bottom furnace and adopt a three-stage heating system for heating, and one-time piercing heating: Preheating section temperature 900-950℃, heating section temperature 1160±20℃, soaking section temperature 1140±10℃, heating speed: 1.5-4min / mm; Secondary piercing heating: preheating section temperature 900-950℃, heating section temperature 1140±20℃, soaking section temperature 1160±10℃, heating speed: 1.5-4min / mm; Step 4: Punching machine deformation: The billet is pierced and deformed twice in the punching machine, billet diameter: 200-300mm, hot rolling parameters are set as follows: First piercing parameter setting: set roller distance: 183-264mm, guide plate distance: 198-285mm; Head front The extension is 33-45mm, the roller speed is 18-30 rpm; the roller bite angle is 10-12°, and the secondary piercing parameters are set: set the roller distance: 188-270mm, the guide plate distance: 230-300mm; the head extension is 40-45mm, the roller speed is 25-30 rpm; the roller bite angle is 10-12°; Step 5: Complete the secondary piercing, the heating speed of the first hot piercing is ≤2mm / min, the heating temperature is 1140±10℃, and the piercing deformation is 40-50%; the heating speed of the second hot piercing is 3-4mm / min, the heating temperature is 1160±10℃, and the piercing deformation is 30-40%.
[0006] The requirements for drilling in step 2 are: centering hole size: d=0.2*D, D: blank diameter, tolerance is ±1mm; centering hole depth h=50-100mm, tolerance is ±1mm; the centering hole is required to be smooth and burr-free, concentricity: ≤1mm.
[0007] Step 3: During heating, the blank is turned 175° to 185° in the circumferential direction every 8 to 10 minutes.
[0008] The beneficial effects of the present invention are as follows: for the production method of hot perforation of NO8810 iron-nickel-based alloy tubes, compared with the production of thick-walled tubes with an outer diameter / wall thickness of ≤10 by one-time hot perforation, the present invention adjusts the deformation amount of the hot perforation pass to perform secondary perforation to obtain a thin-walled NO8810 nickel-based alloy seamless steel tube with a diameter-to-wall ratio of >13, which has the following effects: the perforation method of the present invention reduces the number of subsequent cold processing production passes of the nickel-based NO8810 alloy tube and improves the yield rate. DETAILED DESCRIPTION
[0009] In view of the fact that the hot rolling deformation is small during the perforation production of the iron-nickel-based alloy tube due to the hot working strength, the produced iron-nickel-based alloy tube has a thick-walled tube with a diameter-to-wall ratio of ≤10, which causes a series of problems such as an increase in subsequent cold expansion / rolling passes, repeated heat treatment, an increase in process passes, and increased energy consumption. The present invention provides a manufacturing method for secondary perforation forming of a NO8810 iron-nickel-based alloy large-diameter thin-walled seamless tube. The main innovation is that a secondary hot rolling deformation method is adopted. By reasonably allocating the hot rolling deformation amount of each pass, adjusting the perforation rolling parameters for each time and the secondary perforation heating system, a large-diameter thin-walled seamless iron-nickel-based alloy tube with a diameter-to-wall ratio of >13 can be produced.
[0010] Specifically, the present invention is implemented by a mushroom-type piercing machine. The difficulty lies in the principle of each deformation amount distribution. (1) The secondary hot piercing deformation method is adopted to reasonably distribute the hot piercing deformation amount of each pass. The first hot piercing deformation amount: 40-50%, the second hot piercing deformation amount: 30-40%, and the thin-walled nickel-based NO8810 alloy tube with a diameter-to-wall ratio of >13 is produced. (2) Two hot rolling piercings are adopted to control the temperature and heating time of the first heating and the second heating: in the first heating process, since the billet is solid round steel, the heating speed should be slow to ensure that the temperature inside and outside the billet is uniform. The preheating section furnace temperature: ≥800℃, the soaking section furnace temperature: 1160±20℃, the heating speed is 1.5-2min / mm; in the second heating process, since the billet is a hollow seamless tube, the heating speed should be fast to prevent the temperature difference between the inner and outer surfaces, and the heating speed is 3-4min / mm. Adjust the rolling parameters of the piercing machine each time and the heating system for the second piercing to ensure that the tube billet is smoothly "bite-in" and the piercing is completed. (3) Adjustment of piercing parameters; Due to the different states of the billet during the first piercing and the second piercing, the roller reduction and the guide plate ovality are as follows: first piercing: roller reduction 8-8.5%, guide plate ovality: 1.08-1.1; second piercing: roller reduction 10-10.5%, guide plate ovality: 1.18-1.22.
[0011] The specific implementation steps are as follows: 1. Billet requirements: The billet should be subjected to electroslag remelting + radial forging + turning + ultrasonic inspection.
[0012] 2. Billet processing: 2.1 Billet peeling: To ensure the surface quality, the billet is required to be peeled, the peeling amount is 1.5-2mm on one side, and the surface roughness after peeling is Ra<4μm; 2.2 Billet sawing: sawing and cutting according to the process requirements, the deviation of the vertical line between the section and the billet axis after sawing is ≤3mm. 2.3 Billet centering: punching at the center of the billet can prevent the end of the rough pipe from being "eccentric" and reduce the axial resistance of hot rolling piercing, and prevent "rolling jam". The size of the centering hole is d=0.2*D (billet diameter), and the tolerance is ±1mm; the depth of the centering hole is h=50-100mm, and the tolerance is ±1mm; the centering hole is required to be smooth and burr-free, and the concentricity is ≤1mm.
[0013] 3. Billet heating: Because it is a secondary piercing process, in order to make the heating temperature distribution of billets in different states uniform, the billets in different states are placed in an inclined bottom furnace and heated by a three-stage heating system. The preheating section temperature is ≥900±30℃, the heating temperature is 1160±20℃, the heating speed range is: 1.5-4min / mm, and the soaking section temperature is 1140±10℃. Main heating operation points: turn the billet 175°~185° along the circumferential direction every 8~10 minutes.
[0014] 4. Deformation of the puncher: The billet needs to be deformed by "twice" punching in the mushroom puncher. The deformation mechanism is that the roller and the guide plate form a closed cavity in cross section, and the roller with a rolling angle of 15° above and below provides axial movement and rotational movement. Under the action of the molybdenum-based plug, the rod gradually forms a tube. The various rolling process parameters in the punching process should be strictly controlled and set. The main process parameters are the roller spacing, guide plate spacing, plug extension, roller speed and other process parameters. The parameters of the piercing machine are adjusted according to different specifications of the billet. In the present invention, the billet diameter is D=200 mm, and the hot rolling parameters are set as follows: the first piercing parameter setting is as follows: the roll distance is set to d=183 mm, the guide plate distance is set to b=198 mm; the plug extension is 33 mm, the roll speed is 25 rpm; the roll bite angle is 10°, and the second piercing parameter setting is as follows: the roll distance is set to d=188 mm, the guide plate distance is set to b=230 mm; the plug extension is 40 mm, the roll speed is 28 rpm; and the roll bite angle is 12°.
[0015] 5. Complete the piercing: Due to the different states of the billet for the first and second piercing, the heating process and the piercing process are different. The heating process needs to avoid the temperature difference between the inner and outer holes of the billet, and strictly control the heating speed of the first heating and the second heating. The first heating speed is ≤2mm / min, and the second heating speed is 3-4mm / min; the piercing process needs to balance the head torque and control the piercing speed to prevent adhesion and scratching. Especially for the second piercing, since the tube billet is a "thick-walled tube", in order to prevent heating defects and smooth production of the piercing machine, the parameters of the piercing machine are reset, and the parameters of the second piercing are set: set the roll distance: d=188 mm, the guide plate distance: b=230 mm; the head extension is 40mm, the roll speed is 28 rpm; the roll bite angle is 12°. By increasing the roll pressure and the guide plate ovality, the second piercing process is completed, and the nickel-based NO8810 alloy tube with a diameter-to-wall ratio of >13 is successfully produced.
[0016] In order to fully understand the purpose, characteristics and effects of the present invention, the present invention is described in detail through the following specific embodiments. Example 1 Using the manufacturing method of the present invention
[0017] (1) Billet processing: The billet material is NO8810 forging billet; the outer surface roughness of the billet is Ra<4μm; the deviation of the saw cut surface from the vertical line of the billet axis is ≤3mm. In order to reduce the rolling force during piercing, a centering hole is punched at the end, with a diameter of Φ50mm and a depth of 80mm; concentricity: ≤1mm; the outer diameter of the billet after processing is 200mm.
[0018] (2) Billet heating: Primary heating: Place the processed billet in a three-stage heating system of an inclined bottom furnace for heating, so that the billet is heated evenly and is heated to 1160°C before being taken out of the furnace (operation points: turn the billet 175° to 185° in the circumferential direction every 8 to 10 minutes).
[0019]
[0020] Secondary heating: Place the nickel-based NO8810 alloy tube that has been pierced once in a three-stage heating system in an inclined bottom furnace for heating until it reaches 1160°C and then take it out of the furnace (operation points: turn the billet 175°~185° in the circumferential direction every 8~10 minutes).
[0021]
[0022] (3) Punching machine parameter setting: The punching of NO8810 raw material after heating and insulation is carried out on the punching machine with the mold clamped after parameter setting; parameter setting (tube diameter: 200mm, primary punching specification 210*30mm, secondary punching specification 250*15mm); primary punching parameter setting: set the roll distance: d=183mm, guide plate distance: b=198mm; the head extension is 33mm, the roll speed is 25 rpm; the roll bite angle is 10°; secondary punching parameter setting: set the roll distance: d=188mm, guide plate distance: b=230mm; the head extension is 40mm, the roll speed is 28 rpm; the roll bite angle is 10°.
[0023] (4) Complete secondary piercing: When perforating the tube billet, first perforate once, with the perforation specification of 210*30mm, and then inspect the inner and outer surfaces of the 210*30mm nickel-based NO8810 alloy seamless tube, and grind it to ensure that the tube billet is free of defects during the secondary piercing. Then, the 210*30mm nickel-based NO8810 tube is heated and perforated for the second time to produce a 250*15mm thin-walled nickel-based NO8810 alloy seamless tube, with a seamless tube diameter-to-wall ratio of 16.6>13. Only one cold processing is required to produce the finished product, and the yield rate is increased by 2.5-3.5%. Example 2: Using the original manufacturing method
[0024] (1) Billet processing: The billet material is NO8810 forging billet; the outer surface roughness of the billet is Ra<4μm; the deviation of the saw cut surface from the vertical line of the billet axis is ≤3mm. In order to reduce the rolling force during piercing, a centering hole is punched at the end, with a diameter of Φ50mm and a depth of 80mm; concentricity: ≤1mm; the outer diameter of the billet after processing is 200mm.
[0025] (2) Billet heating: Place the processed billet in a three-stage heating system in an inclined bottom furnace for heating, so that the billet is heated evenly and is heated to 1160°C before being taken out of the furnace (operation points: turn the billet 175° to 185° in the circumferential direction every 8 to 10 minutes).
[0026]
[0027] (3) Punching machine parameter setting: The punching of the NO8810 raw material after heating and insulation is carried out on the punching machine with the mold clamped after parameter setting; parameter setting (tube diameter: 200 mm, punching specification 210*20 mm); punching parameter setting: set the roll distance: d=183 mm, guide plate distance: b=198 mm; the head extension is 45 mm, the roll speed is 27 rpm; the roll bite angle is 10°.
[0028] (4) Complete the piercing: The tube billet is pierced normally, the piercing specification is: 210*20mm, and then the inner and outer surfaces of the 210*20mm nickel-based NO8810 alloy seamless tube are inspected. After grinding and turning to the cold line, it needs to be cold expanded 2 times + 1 time cold rolling to produce the finished product, and the yield rate is reduced by 2.5-3.5%.
[0029] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.
Claims
1. A method for manufacturing a large-diameter thin-walled seamless iron-nickel alloy tube, characterized in that: The following steps are involved: Step 1: Billet requirements: For the billet, electroslag remelting + radial forging + turning + ultrasonic inspection are used. The chemical composition requirements of the billet are: C: 0.06-0.1%, Si≤1%, Mn: 1.0-1.5%, P≤0.01%, S≤0.01%, Cr: 19-23%, Ni: 30-35%, Cu: 0.5-0.75%, Fe: 39.5-47%, Al: 0.15-0.6%, Ti: 0.15-0.6%; Size requirements: For billets of φ200mm-300mm, the outer diameter tolerance is -1.8 / +0mm; Ultrasonic inspection: For billets of φ200mm-300mm, the maximum flat-bottom hole diameter corresponding to the flaw detection sensitivity is φ3mm; Step 2: Billet processing: Billet peeling: Peel the billet, the peeling amount is 1.5-2mm on one side, and the surface roughness after peeling is Ra<4μm; Billet sawing: Saw the billet, and the deviation of the vertical line between the cross section and the billet axis after sawing is ≤3mm; Billet centering: Punch a hole at the center of the billet, and the diameter of the hole is 20-80mm; Step 3: Billet heating: Place the billet in an inclined bottom furnace and heat it in a three-stage heating system. The first perforation heating: preheating section temperature 900-950℃, heating section temperature 1160±20℃, soaking section temperature 1140±10℃, heating speed: 1.5-4min / mm; the second perforation heating: preheating section temperature 900-950℃, heating section temperature 1140±20℃, soaking section temperature 1160±10℃, heating speed: 1.5-4min / mm; Step 4: Punching machine deformation: The billet is punched and deformed twice in the punching machine, the billet diameter is 200-300mm, and the hot rolling parameters are set as follows: the first punching parameter setting: set the roll distance: 183-264mm, the guide plate distance: 198-285mm; the head extension is 33-45mm, the roll speed is 18-30 rpm; the roll bite angle is 10-12°, the second punching parameter setting: set the roll distance: 188-270mm, the guide plate distance: 230-300mm; the head extension is 40-45mm, the roll speed is 25-30 rpm; the roll bite angle is 10-12°; Step 5: Complete the secondary perforation. The heating speed of the first hot perforation is ≤2mm / min, the heating temperature is 1140±10℃, and the perforation deformation is 40-50%. The heating speed of the second hot perforation is 3-4mm / min, the heating temperature is 1160±10℃, and the perforation deformation is 30-40%.
2. The method for manufacturing a large-diameter thin-walled seamless iron-nickel alloy pipe according to claim 1, characterized in that: The requirements for drilling in step 2 are: centering hole size: d=0.2*D, D: blank diameter, tolerance is ±1mm; centering hole depth h=50-100mm, tolerance is ±1mm; the centering hole is required to be smooth and burr-free, concentricity: ≤1mm.
3. The method for manufacturing a large-diameter thin-walled seamless iron-nickel alloy pipe according to claim 1, characterized in that: Step 3: During heating, the blank is turned 175° to 185° in the circumferential direction every 8 to 10 minutes.
Citation Information
Patent Citations
Production process of stainless steel rough pipe
CN102274870A
Production method of phi 762 * 48 mm large-diameter nickel-based alloy seamless tube for oil refining device
CN112453100A
Manufacturing method of seamless titanium pipe with radius-thickness ratio larger than 30
CN117718354A
Iron-nickel-based alloy pipe, preparation method and application of iron-nickel-based alloy pipe in preparation of polycrystalline silicon reduction furnace
CN118143579A
Method for manufacturing seamless steel pipe made of high Cr-high Ni alloy steel
US20100000281A1