Preparation method of superfine cobalt powder

The integration of extraction and back extraction processes with vacuum cracking produces ultrafine cobalt powder with desired particle size and morphology, addressing safety and size issues in existing methods, enabling efficient industrial production.

CN119076967APending Publication Date: 2024-12-06GANZHOU NONFERROUS METALLURGICAL RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411205452.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for preparing ultrafine cobalt powder, such as hydrogen reduction, pose safety hazards due to the use of hazardous hydrogen and result in larger particle sizes, particularly with vacuum cracking of cobalt oxalate powder, which does not achieve the desired ultrafine particle size of 0.1 to 1.0 μm.

Method used

A method involving the integration of extraction and back extraction processes using a composite extractant, phase modifier, and oxalate-containing stripping agent to produce ultrafine cobalt oxalate powder, followed by cracking under vacuum and/or inert atmosphere to obtain ultrafine cobalt powder with a particle size of 0.1 to 1.0 μm.

Benefits of technology

The method achieves ultrafine cobalt powder with a quasi-spherical morphology and good fluidity, eliminating safety hazards associated with hydrogen use and providing a cost-effective, simple preparation process suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076967A_ABST
    Figure CN119076967A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of superfine cobalt powder, and relates to the technical field of metallurgy. The preparation method of the superfine cobalt powder comprises the following steps that a cobalt-containing solution and an organic extraction agent are mixed and extracted, and a cobalt-containing extraction phase is obtained; mixing the cobalt-containing extraction phase with a stripping agent, performing stripping, and performing solid-liquid separation to obtain superfine cobalt oxalate powder; the stripping agent comprises a stabilizer and an oxalate-containing aqueous solution; the particle size of the superfine cobalt oxalate powder is 0.2 to 1.5 microns; and the superfine cobalt oxalate powder is cracked, and the superfine cobalt powder is obtained. The cracking is carried out in a vacuum and / or inert atmosphere; the particle size of the superfine cobalt powder is 0.1-1 [mu] m. According to the method, the cobalt oxalate ultrafine powder is prepared and purified by adopting an extraction and back extraction separation preparation integrated technology, so that the process is simple, the reagent consumption is low, and the cost is low; and secondly, a hydrogen reduction technology is replaced by cracking, and the prepared superfine cobalt powder is in a sphere-like shape and is good in fluidity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for preparing ultrafine cobalt powder. Background Art

[0002] Ultrafine cobalt powder is widely used in cemented carbide, battery, hydrogen energy, chemical reaction catalysis, magnetic materials and other fields due to its high specific surface area, catalytic activity, hydrogen storage capacity and recycling performance. The use of ultrafine cobalt powder to prepare cemented carbide can not only reduce its porosity and avoid the appearance of cobalt pools, but also a layer of cobalt adheres to the surface of WC particles, which is conducive to separating WC grains, all of which are conducive to improving the comprehensive performance of cemented carbide. In recent years, due to the rapid development of the battery industry, the use of ultrafine cobalt powder in the battery industry has increased sharply.

[0003] In the prior art, the preparation method of ultrafine cobalt powder is mainly hydrogen reduction method, and other preparation methods such as hydrazine hydrate method, gas phase method, sol-gel method, etc. have not been industrialized. For example, China CN106346021A discloses a method for preparing cobalt powder by high-pressure hydrogen reduction, wherein a dispersant is added to a cobalt salt aqueous solution, ammonia water is added thereto after mixing evenly, and ultrafine cobalt powder is obtained by hydrogen reduction under conditions of 140-220°C and 2.0-3.8MPa. China patent CN113172233A discloses a nano-spherical close-packed hexagonal cobalt powder and a preparation method thereof, wherein sodium borohydride is used as a catalyst to convert soluble Cobalt salt, dispersant and ammonia water are made into slurry, and high-pressure hydrogen reduction reaction is carried out at 220-350°C and 3.8-5.5MPa to prepare ultrafine cobalt powder with an average particle size of ≤400nm; Chinese patent CN101653830A discloses a method for preparing ultrafine cobalt powder with a close-packed hexagonal structure or a face-centered cubic structure by hydrogen reduction. By adding PdCl2 as a catalyst, hydrogen reduction is carried out at 180°C and 1.0MPa to obtain ultrafine cobalt powder with a particle size of 200nm, which greatly reduces the hydrogen pressure. However, this patent requires a secondary reduction process, and the secondary reduction temperature is as high as 400-700°C.

[0004] Since hydrogen is a hazardous source during the hydrogen reduction process, there are safety hazards in the preparation process of ultrafine cobalt powder using hydrogen reduction technology. For this reason, in the prior art, ultrafine cobalt powder is prepared by vacuum cracking cobalt oxalate powder, wherein the cobalt oxalate powder is usually prepared by directly precipitating a soluble technical cobalt salt and an oxalate. The cobalt oxalate powder prepared by this method has a larger particle size, and the particle size of the ultrafine cobalt powder obtained after cracking is about 2.5 μm, and there is still a defect that the ultrafine cobalt powder has a larger particle size. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing ultrafine cobalt powder. The present invention prepares ultrafine cobalt oxalate powder through an integrated separation and preparation technology of extraction and back extraction, and obtains ultrafine cobalt powder with a particle size of 0.1 to 1.0 μm after cracking.

[0006] In order to achieve the purpose of the present invention, the present invention provides the following technical solutions:

[0007] A method for preparing ultrafine cobalt powder comprises the following steps:

[0008] mixing the cobalt-containing solution and the organic extractant, extracting, and obtaining a cobalt-containing extract phase;

[0009] The cobalt-containing extract phase and the stripping agent are mixed, stripped, and solid-liquid separated to obtain ultrafine cobalt oxalate powder; the stripping agent includes a stabilizer and an oxalate-containing aqueous solution; the particle size of the ultrafine cobalt oxalate powder is 0.2 to 1.5 μm;

[0010] The ultrafine cobalt oxalate powder is cracked to obtain the ultrafine cobalt powder; the cracking is performed under vacuum and / or inert atmosphere; the particle size of the ultrafine cobalt powder is 0.1-1 μm.

[0011] Preferably, the source of cobalt in the cobalt-containing solution is cobalt salt; and the concentration of cobalt in the cobalt-containing solution is 0.01 to 3 mol / L.

[0012] Preferably, the organic extractant comprises a composite extractant, a phase modifier and a diluent; the volume ratio of the composite extractant, the phase modifier and the diluent is 1:0.05-0.3:1-10.

[0013] Preferably, the composite extractant comprises an ammonia extractant and a carboxylic acid extractant;

[0014] The phase modifier is an alkanol having 4 to 10 carbon atoms;

[0015] The diluent includes one or more of alkanes with carbon atoms of 5 to 16, kerosene and paraffin.

[0016] Preferably, the volume ratio of the ammonia extractant to the carboxylic acid extractant is 0.5 to 10:1.

[0017] Preferably, the flow ratio of the cobalt-containing solution to the organic extractant is 1:0.1-10.

[0018] Preferably, the concentration of oxalate in the aqueous oxalate-containing solution is 1 to 100 g / L; and the volume ratio of the stabilizer to the aqueous oxalate-containing solution is 0.01 to 0.50:1.

[0019] Preferably, the stabilizer comprises one or more of ethylene glycol, glycerol and tetraethylene glycol;

[0020] The source of oxalate in the aqueous oxalate-containing solution includes oxalic acid or oxalate.

[0021] Preferably, the extraction stages are 1 to 20.

[0022] Preferably, the cracking temperature is 300-600° C., the time is 0.5-10 h, and the vacuum degree is 1-1000 Pa.

[0023] The invention provides a method for preparing ultrafine cobalt powder, comprising the following steps: mixing a cobalt-containing solution and an organic extractant, extracting to obtain a cobalt-containing extraction phase; mixing the cobalt-containing extraction phase and a stripping agent, stripping, and obtaining ultrafine cobalt oxalate powder after solid-liquid separation; the stripping agent comprises a stabilizer and an oxalate-containing aqueous solution; the particle size of the ultrafine cobalt oxalate powder is 0.2-1.5 μm; cracking the ultrafine cobalt oxalate powder to obtain the ultrafine cobalt powder; the cracking is performed under vacuum and / or inert atmosphere; the particle size of the ultrafine cobalt powder is 0.1-1 μm. The invention purifies cobalt through an extraction process on the one hand, and obtains a cobalt-containing loaded organic phase on the other hand; the cobalt-containing loaded organic phase forms a microemulsion reactor with an oxalate-containing aqueous solution during the back extraction process, and in the microemulsion reactor, cobalt ions combine with oxalate ions to form molecular cobalt oxalate, and the molecular cobalt oxalate demulsifies and enters the aqueous phase, and is coated by a stabilizer to prevent the growth of cobalt oxalate molecules, thereby obtaining ultrafine cobalt oxalate powder, and the preparation process is simple and the cost is low; secondly, the invention adopts cracking under vacuum and / or inert atmosphere to replace hydrogen reduction technology, eliminates the use of hydrogen as a dangerous source, and has good safety; the prepared ultrafine cobalt powder has a quasi-spherical morphology and good fluidity. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0025] Figure 1 This is the SEM image of the ultrafine cobalt powder obtained in Example 1. DETAILED DESCRIPTION

[0026] The present invention provides a method for preparing ultrafine cobalt powder, comprising the following steps:

[0027] mixing the cobalt-containing solution and the organic extractant, extracting, and obtaining a cobalt-containing extract phase;

[0028] The cobalt-containing extract phase and the stripping agent are mixed, stripped, and solid-liquid separated to obtain ultrafine cobalt oxalate powder; the stripping agent includes a stabilizer and an oxalate-containing aqueous solution; the particle size of the ultrafine cobalt oxalate powder is 0.2 to 1.5 μm;

[0029] The ultrafine cobalt oxalate powder is cracked to obtain the ultrafine cobalt powder; the cracking is performed under vacuum and / or inert atmosphere; the particle size of the ultrafine cobalt powder is 0.1-1 μm.

[0030] In the present invention, unless otherwise specified, all preparation raw materials are preferably commercially available products well known to those skilled in the art.

[0031] The present invention mixes a cobalt-containing solution and an organic extractant, extracts, and obtains a cobalt-containing extraction phase. In the present invention, the source of cobalt in the cobalt-containing solution is preferably one or more of cobalt salts, metallic cobalt, and cobalt-containing minerals, more preferably cobalt salts; the cobalt salt is preferably one or more of cobalt chloride, cobalt sulfate, cobalt nitrate, cobalt formate, and cobalt acetate, more preferably cobalt chloride, cobalt sulfate, or cobalt nitrate; the concentration of cobalt in the cobalt-containing solution is preferably 0.01 to 3 mol / L, more preferably 1 to 3 mol / L; the cobalt-containing solution also preferably includes a regulator; the regulator is preferably nitric acid.

[0032] In the present invention, the organic extractant preferably includes a composite extractant, a phase modifier and a diluent; the composite extractant preferably includes an ammonia extractant and a carboxylic acid extractant; the ammonia extractant is preferably one or more of tri(octyl-decyl)alkyl tertiary amine extractant (N235), secondary carbon primary amine extractant (N1923) and trioctylmethylammonium chloride (N263), more preferably N235; the carboxylic acid extractant is preferably one or more of cycloalkane acid, isomeric acid (Versatic911), secondary octylphenoxy substituted acetic acid (CA-12) and secondary nonylphenoxy substituted acetic acid (CA-100), more preferably isomeric acid or cycloalkane acid; the volume ratio of the carboxylic acid extractant to the ammonia extractant is preferably 0.5-10:1, more preferably 1-3:1.

[0033] In the present invention, the phase modifier is preferably an alkanol having 4 to 10 carbon atoms; the alkanol is preferably a branched alkanol or a branched alkanol, more preferably n-octanol, sec-octanol, isooctyl alcohol or 2-methylheptanol, further preferably sec-octanol or 2-methylheptanol.

[0034] In the present invention, the diluent preferably includes one or more of alkanes with carbon numbers of 5 to 16, kerosene and paraffin, and is more preferably kerosene; the alkanes with carbon numbers of 5 to 16 preferably include substituted alkanes with carbon numbers of 5 to 16 or unsubstituted alkanes with carbon numbers of 5 to 16; the substituted alkanes with carbon numbers of 5 to 16 include alicyclic alkanes with carbon numbers of C5 to C16 or aromatic hydrocarbons with carbon numbers of C6 to C10; the kerosene is preferably aviation kerosene or sulfonated kerosene, and is more preferably sulfonated kerosene; the paraffin is preferably liquid paraffin.

[0035] In the present invention, the volume ratio of the organic extractant, the phase modifier and the diluent is preferably 1:0.05-0.5:1-10, and more preferably 1:0.30-0.4:1.25-3.

[0036] In the present invention, the flow ratio of the cobalt-containing solution to the extractant is preferably 1:0.1-10, more preferably 1:2-5.

[0037] In the present invention, the number of extraction stages is preferably 1 to 20, more preferably 2 to 10, and further preferably 3 to 6; the temperature of the extraction is preferably room temperature, and the time is preferably 5 to 60 minutes, and more preferably 10 to 20 minutes. The present invention uses extraction to obtain a loaded organic phase and to purify the solution, and removes trace amounts of impurity ions such as Ca, Mg, Cu, Zn, Ni, Na, and K in the solution.

[0038] In the present invention, after the extraction, the obtained cobalt-containing extract phase is preferably washed; the washing agent used in the washing is preferably one or more of nitric acid, sulfuric acid and hydrochloric acid, more preferably nitric acid; the acidity of the washing agent is preferably 0.1-6 mol / L, more preferably 0.2-3 mol / L, based on the molar concentration of hydrogen ions; the flow ratio of the cobalt-containing extract phase to the washing agent is preferably 1:0.1-5 mL / min, more preferably 1:0.1-1 mL / min; the number of washing stages is preferably 0-10, more preferably 1-4, and further preferably 2-3.

[0039] After obtaining the cobalt-containing extraction phase, the present invention mixes the cobalt-containing extraction phase with a stripping agent, performs stripping, and obtains the ultrafine cobalt oxalate powder after solid-liquid separation.

[0040] In the present invention, the stripping agent preferably includes a stabilizer and an oxalate-containing aqueous solution; the source of oxalate in the oxalate-containing aqueous solution includes oxalic acid or oxalate, more preferably oxalic acid; the oxalate is preferably one or more of ammonium oxalate, sodium oxalate and potassium oxalate; the stabilizer preferably includes one or more of ethylene glycol, propylene glycol and tetraethylene glycol, more preferably ethylene glycol; the concentration of oxalate in the oxalate-containing aqueous solution is preferably 1 to 100 g / L, more preferably 80 to 100 g / L; the volume ratio of the stabilizer to the oxalate-containing aqueous solution is preferably 0.01 to 0.50:1, more preferably 0.10 to 0.25:1.

[0041] In the present invention, the stripping temperature is preferably room temperature, the time is preferably 5 to 30 minutes; the stripping is preferably carried out under ultrasonic and / or stirring conditions; the ultrasonic frequency is preferably 10 to 90 Hz, more preferably 30 to 80 Hz; the stirring rate is preferably 50 to 300 rpm, more preferably 100 to 200 rpm. The present invention removes non-cobalt metal ion impurities through stripping to prepare ultrafine cobalt oxalate powder.

[0042] In the present invention, the chemical reaction equations in the extraction and stripping processes are as follows:

[0043] Co 2+ (a) +HA·L (O) →Co(A·L) 2(O) +2H + (a) ;

[0044] Co(A·L) 2(O) +H2C2O 4(a) →CoC2O4↓+2HAL (O) ;

[0045] Here, a represents the aqueous phase and o represents the organic phase.

[0046] In the present invention, the solid-liquid separation method is preferably filtration, suction filtration or centrifugation; the present invention also preferably dries the solid phase after solid-liquid separation to obtain the cobalt oxalate powder; the drying temperature is preferably 20 to 200°C, more preferably 100 to 190°C; the drying time is preferably 1 to 5 hours, more preferably 2 to 3 hours.

[0047] In the present invention, the particle size of the ultrafine cobalt oxalate powder is 0.2 to 1.5 μm, preferably 0.6 to 1.0 μm.

[0048] After obtaining the ultrafine cobalt oxalate powder, the present invention cracks the ultrafine cobalt oxalate powder to obtain the ultrafine cobalt powder.

[0049] In the present invention, the cracking is carried out under vacuum and / or inert atmosphere; the inert atmosphere preferably includes argon or nitrogen, more preferably argon; the vacuum degree of the vacuum is preferably 1-1000 Pa, more preferably 1-100 Pa; the cracking temperature is preferably 300-600°C, more preferably 400-500°C; the time is preferably 0.5-10h, more preferably 2-5h, and the vacuum degree is preferably 1-1000 Pa, more preferably 1-100 Pa.

[0050] In the present invention, the particle size of the ultrafine powder is 0.1 to 1 μm, preferably 0.3 to 0.5 μm.

[0051] In order to further illustrate the present invention, the preparation method of the ultrafine cobalt powder provided by the present invention is described in detail below in conjunction with examples, but they should not be construed as limiting the scope of protection of the present invention.

[0052] Example 1

[0053] Nitric acid was used as a regulator and commercially available cobalt nitrate was used as a raw material to prepare Co 2+ 10L of cobalt nitrate solution with a concentration of 0.2mol / L and a pH value of 4.5; 10L of extractant prepared with 2L of cyclohexane acid, 2L of N235, 1L of octanol and 5L of sulfonated kerosene; 5L of nitric acid with a concentration of 0.1mol / L as the detergent; 5L of stripping agent prepared with 1L of ethylene glycol, 0.4Kg of oxalic acid and 4L of ultrapure water;

[0054] An 8-stage 1L mixed clarification extraction tank (including 6-stage extraction and 2-stage washing) was used, and the flow ratio of the extractant, the cobalt nitrate solution and the washing liquid in the extraction tank was 50:25:5 mL / min, and extraction was performed at room temperature to obtain a cobalt-containing extract phase;

[0055] 1L of cobalt-containing extract phase was mixed with 0.5L of stripping agent, stripped for 30min under ultrasonic and stirring conditions, and solid phase cobalt oxalate was obtained after centrifugation;

[0056] The cobalt oxalate powder was dried at 100° C. for 2 h to obtain 18 g of cobalt oxalate powder, which was then transferred into a tube furnace and cracked for 2 h in an argon atmosphere at 400° C. and 10 Pa to obtain 8.5 g of ultrafine cobalt powder with a particle size of 0.5 μm and a purity of 99.9991%.

[0057] Figure 1 This is the SEM image of the ultrafine cobalt powder obtained in Example 1. Figure 1 It can be seen that the ultrafine cobalt powder prepared by the present invention has a spherical morphology and has good fluidity.

[0058] Example 2

[0059] Nitric acid was used as a regulator and commercially available cobalt chloride was used as a raw material to prepare Co 2+10L of cobalt chloride solution with a concentration of 0.2mol / L and a pH value of 4.5; 10L of extractant prepared with 2L of cyclohexane acid, 2L of N235, 1L of octanol and 5L of sulfonated kerosene; 5L of nitric acid with a concentration of 0.1mol / L as the detergent; 5L of stripping agent prepared with 1L of ethylene glycol, 0.4Kg of oxalic acid and 4L of ultrapure water;

[0060] A 5-stage 1L mixed clarification extraction tank (including 3-stage extraction and 2-stage washing) was used, the flow ratio of the extractant, the cobalt chloride solution and the washing liquid in the extraction tank was 50:25:15 mL / min, and extraction was performed at room temperature to obtain a cobalt-containing extract phase;

[0061] 1L of cobalt-containing extract phase was mixed with 0.5L of stripping agent, stripped for 30min under ultrasonic and stirring conditions, and solid phase cobalt oxalate was obtained after centrifugation;

[0062] The cobalt oxalate powder was dried at 100°C for 2 hours to obtain 18 g of cobalt oxalate powder, which was then transferred into a tube furnace and cracked for 2 hours in an argon atmosphere at 400°C and 1000 Pa to obtain 8.2 g of ultrafine cobalt powder with a particle size of 0.3 μm and a purity of 99.9993%.

[0063] Example 3

[0064] Nitric acid was used as a regulator and commercially available cobalt sulfate was used as a raw material to prepare Co 2+ 10L of cobalt sulfate solution with a concentration of 0.2mol / L and a pH value of 4.5; 10L of extractant prepared with 3L of isomeric acid (V911), 1L of N263, 1.5L of 2-methylheptanol and 4.5L of sulfonated kerosene; 5L of nitric acid with a concentration of 0.1mol / L as the detergent; 5L of stripping agent prepared with 1L of ethylene glycol, 0.4Kg of oxalic acid and 4L of ultrapure water;

[0065] A 7-stage 1L mixed clarification extraction tank (including 6-stage extraction and 1-stage washing) was used, the flow ratio of the extractant, the cobalt sulfate solution and the washing liquid in the extraction tank was 50:25:15 mL / min, and extraction was performed at room temperature to obtain a cobalt-containing extract phase;

[0066] 1L of cobalt-containing extract phase was mixed with 0.5L of stripping agent, stripped for 30min under ultrasonic and stirring conditions, and solid phase cobalt oxalate was obtained after centrifugation;

[0067] The cobalt oxalate powder was dried at 200° C. for 2 h to obtain 18 g of cobalt oxalate powder, which was then transferred into a tube furnace and cracked at 400° C. for 2 h in an argon atmosphere to obtain 8.7 g of ultrafine cobalt powder with a particle size of 0.3 μm and a purity of 99.9990%.

[0068] The above examples prove that the present invention adopts cracking under vacuum and / or inert atmosphere instead of hydrogen reduction to prepare ultrafine cobalt powder, and obtains ultrafine cobalt powder with a particle size of 0.1 to 1.0 μm, eliminates the use of dangerous source hydrogen, and has a simple preparation method and can be used for industrial production.

[0069] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing ultrafine cobalt powder, characterized in that: The following steps are involved: mixing the cobalt-containing solution and the organic extractant, extracting, and obtaining a cobalt-containing extract phase; The cobalt-containing extract phase and the stripping agent are mixed, stripped, and solid-liquid separated to obtain ultrafine cobalt oxalate powder; the stripping agent includes a stabilizer and an oxalate-containing aqueous solution; the particle size of the ultrafine cobalt oxalate powder is 0.2 to 1.5 μm; The ultrafine cobalt oxalate powder is cracked to obtain the ultrafine cobalt powder; the cracking is performed under vacuum and / or inert atmosphere; the particle size of the ultrafine cobalt powder is 0.1-1 μm.

2. The preparation method according to claim 1, characterized in that: The source of cobalt in the cobalt-containing solution is cobalt salt; the concentration of cobalt in the cobalt-containing solution is 0.01-3 mol / L.

3. The preparation method according to claim 1, characterized in that: The organic extractant comprises a composite extractant, a phase modifier and a diluent; the volume ratio of the composite extractant, the phase modifier and the diluent is 1:0.05-0.3:1-10.

4. The preparation method according to claim 3, characterized in that: The composite extractant includes an ammonia extractant and a carboxylic acid extractant; The phase modifier is an alkanol having 4 to 10 carbon atoms; The diluent includes one or more of alkanes with carbon atoms of 5 to 16, kerosene and paraffin.

5. The preparation method according to claim 4, characterized in that: The volume ratio of the ammonia extractant to the carboxylic acid extractant is 1:0.5-10.

6. The preparation method according to any one of claims 2 to 5, characterized in that: The flow ratio of the cobalt-containing solution to the organic extractant is 1:0.1-10.

7. The preparation method according to claim 1, characterized in that: The concentration of oxalate in the aqueous solution containing oxalate is 1-100 g / L; the volume ratio of the stabilizer to the aqueous solution containing oxalate is 0.01-0.50:

1.

8. The preparation method according to claim 1 or 7, characterized in that: The stabilizer includes one or more of ethylene glycol, propylene glycol and tetraethylene glycol; The source of oxalate in the aqueous oxalate-containing solution includes oxalic acid or oxalate.

9. The preparation method according to claim 1, characterized in that: The extraction stages are 1 to 20.