Preparation method of flexible ammonia gas sensitive material

Through Ca-doped CNF/Al2O3 flexible ammonia sensitive material, the problem of insufficient rigidity and sensitivity of existing ammonia detection materials is solved, and ammonia detection with high sensitivity and environmental stability is achieved. It is suitable for flexible electronic equipment and simplifies the Preparation process and reduce costs.

CN119079928APending Publication Date: 2024-12-06JILIN AGRICULTURAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411096585.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Most of the existing ammonia detection materials are rigid materials, which limits their application in flexible electronic devices. The existing ammonia detection technology has problems of insufficient sensitivity, selectivity and stability.

Method used

Using Ca-doped CNF/Al2O3 flexible ammonia sensitive material, an ammonia sensor with high sensitivity, good flexibility and environmental stability is prepared through solution preparation, electrospinning and heat treatment processes.

Benefits of technology

It achieves high sensitivity, good selectivity and long-term stability at room temperature, and is suitable for ammonia detection in flexible electronic equipment, simplifying the preparation process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079928A_ABST
    Figure CN119079928A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a flexible ammonia gas sensitive material, and belongs to the field of semiconductor sensor materials, and the preparation method comprises the following steps: (1) solution preparation: taking polyacrylonitrile (PAN) and N, N-dimethylformamide (DMF) as precursor solutions, and adding aluminum chloride (AlCl3) and calcium chloride (CaCl2) to obtain a spinning solution; (2) preparing a nanofiber film by adopting an electrostatic spinning technology under the conditions of proper temperature, humidity, voltage, receiving distance and the like; the prepared nanofiber film is subjected to pre-oxidation and carbonization, and the flexible ammonia gas sensitive material-Ca doped CNF / Al2O3 is obtained. The preparation method has the main advantages that (1) the whole preparation process is simple and convenient to operate, and comprises three steps of solution preparation, electrostatic spinning and heat treatment; and (2) the flexible ammonia gas sensitive material is high in sensitivity and stability and has good selectivity and repeatability, and a feasible method is provided for ammonia gas detection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of flexible semiconductor sensor materials, and more specifically, relates to a Ca-doped CNF / Al2O3 flexible ammonia sensitive material. Background Art

[0002] With the increasing attention paid to environmental monitoring and food safety in modern society, the demand for harmful gas detection technology is growing. Ammonia is a common harmful gas that is widely present in industrial emissions, agricultural fertilizers, and certain foods. Therefore, the development of a highly sensitive and highly selective ammonia sensor is of great practical significance.

[0003] At present, ammonia detection technologies mainly include electrochemical sensors, optical sensors and semiconductor sensors. Although these methods can realize the detection of ammonia to a certain extent, they still have some limitations. For example, electrochemical sensors usually require complex sample pretreatment processes and are easily interfered by other gases; the sensitivity and stability of optical sensors are often limited by the optical properties of the material itself; and although semiconductor sensors have good sensitivity, their stability and selectivity still need to be improved.

[0004] In addition, most existing ammonia detection materials are rigid materials, which limits their application in flexible electronic devices. With the development of wearable devices and flexible electronic technology, the demand for flexible sensors is increasing. However, how to combine highly sensitive ammonia detection functions with flexible materials remains a technical challenge. Summary of the invention

[0005] In view of the shortcomings of the prior art or the need for improvement, the present invention provides a flexible sensitive material for monitoring ammonia at room temperature, with a simple overall process and low cost. The ammonia sensor prepared with the sensitive material has high sensitivity, good flexibility, selectivity and environmental stability.

[0006] One object of the present invention is to provide a Ca-doped CNF / Al2O3 flexible ammonia sensitive material, comprising the following preparation steps:

[0007] (1) Solution preparation: Weigh 1.2 g of polyacrylonitrile powder (PAN) and add it to 8.8 g of N,N-dimethylformamide (DMF), and stir it in a water bath magnetic stirrer at 60°C and 150 r / min for 4 h until a uniform precursor solution is obtained. Then add 0.15 g of AlCl3 and 0.15 g of CaCl2, and stir it in a water bath magnetic stirrer at 60°C and 150 r / min for 6 h. After stirring evenly, let it stand for 24 h to degas, and obtain a spinning solution;

[0008] (2) Electrospinning: At a temperature of 20°C and a relative humidity of 40%, add the spinning solution into a syringe, and place the receiving roller 180 mm away from the syringe needle. Connect the positive electrode of the high-voltage power supply to the syringe needle, and the negative electrode to the receiving roller. Set the spinning voltage to 15 kV, the solution advancing speed to 0.5 mL / h, the roller rotation speed to 120 rad / min, and the time to 2 h to obtain a nanofilm material.

[0009] (3) Pre-oxidation: First, put the nanofilm material into an air circulation oven, set the temperature to 60°C, and set the time to 3 hours for preliminary oxidation. The white nanofiber material appears light yellow. Then set the air circulation oven temperature to 200°C and set the time to 2 hours for further oxidation. The nanofiber material appears khaki. Finally, wait for the material to cool down naturally to complete the pre-oxidation.

[0010] (4) Carbonization: The material was placed in a tubular furnace and nitrogen was continuously introduced into the furnace. The temperature was increased linearly from room temperature at 5°C / min. When the temperature was increased to 1050°C and maintained for 1 h, the nanofibers gradually changed from khaki to black, completing the carbonization transformation process. The nitrogen was then introduced to room temperature to obtain a flexible ammonia-sensitive material, Ca-doped CNF / Al2O3.

[0011] Another object of the present invention is to provide a CNF / Al2O3 flexible ammonia sensitive material, which is prepared by the preparation method according to the present invention, and the performance is compared with that of the Ca-doped CNF / Al2O3 flexible ammonia sensitive material;

[0012] The present invention packages the two flexible ammonia sensitive materials into electrodes, which can be tested in an ammonia environment;

[0013] The present invention has the following characteristics and advantages:

[0014] The overall preparation process is simple and easy to operate, including three steps: solution preparation, electrospinning, and heat treatment.

[0015] Flexible ammonia sensitive materials have high sensitivity, strong stability, good selectivity and repeatability, and provide a practical method for the detection of ammonia. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0017] Figure 1 This is a flexible display diagram of the CNF / Al2O3 ammonia sensitive material prepared in Example 1;

[0018] Figure 2This is a scanning electron microscope image (SEM) of the CNF / Al2O3 ammonia sensitive material prepared according to Example 1;

[0019] Figure 3 This is the energy spectrum (EDS) of the CNF / Al2O3 ammonia sensitive material prepared according to Example 1;

[0020] Figure 4 is an X-ray photoelectron spectrum (XPS) of the CNF / Al2O3 ammonia sensitive material prepared according to Example 1;

[0021] Figure 5 The Raman spectrum (Raman) of the CNF / Al2O3 ammonia sensitive material prepared according to Example 1;

[0022] Figure 6 This is a flexible display diagram of the Ca-doped CNF / Al2O3 ammonia sensitive material prepared in Example 2;

[0023] Figure 7 This is a scanning electron microscope image (SEM) of the Ca-doped CNF / Al2O3 ammonia sensitive material prepared according to Example 2;

[0024] Figure 8 This is the energy spectrum (EDS) of the Ca-doped CNF / Al2O3 ammonia sensitive material prepared according to Example 2;

[0025] Fig. 9 This is the X-ray photoelectron spectroscopy (XPS) of the Ca-doped CNF / Al2O3 ammonia sensitive material prepared according to Example 2;

[0026] Fig.10 This is the Raman spectrum (Raman) of the Ca-doped CNF / Al2O3 ammonia sensitive material prepared according to Example 2;

[0027] Fig.11 The dynamic response curve and calibration curve of the CNF / Al2O3 ammonia sensitive material of Example 1 and the Ca-doped CNF / CNF / Al2O3 ammonia sensitive material of Example 2 under ammonia conditions;

[0028] Fig.12 Selectivity test of Ca-doped CNF / Al2O3 ammonia sensitive material prepared in Example 2;

[0029] Fig.13 Cyclic test of the Ca-doped CNF / Al2O3 ammonia sensitive material prepared in Example 2;

[0030] Fig.14 Long-term stability test of the Ca-doped CNF / Al2O3 ammonia sensitive material prepared in Example 2;

[0031] Fig.15 Environmental temperature and humidity test of the Ca-doped CNF / Al2O3 ammonia sensitive material prepared in Example 2. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0033] In the existing technology, the performance of gas-sensitive materials can be optimized by doping with other elements such as Pt and Pd, but the cost is high and the process is complicated. Figures 1 to 15 As shown, the present invention prepares a CNF / Al2O3 flexible ammonia sensitive material, and further prepares a Ca-doped CNF / Al2O3 flexible ammonia sensitive material by doping calcium, thereby improving the response sensitivity of the material to ammonia;

[0034] Example 1

[0035] (1) Solution preparation: Weigh 1.2 g of polyacrylonitrile powder (PAN) and add it to 8.8 g of N,N-dimethylformamide (DMF), and stir it in a water bath magnetic stirrer at 60°C and 150 r / min for 4 h until a uniform precursor solution is obtained. Then add 0.3 g of AlCl3, stir it in a water bath magnetic stirrer at 60°C and 150 r / min for 6 h, stir it evenly and let it stand for 24 h to degas, and obtain a spinning solution;

[0036] (2) Electrospinning: At a temperature of 20°C and a relative humidity of 40%, add the spinning solution into a syringe, and place the receiving roller 180 mm away from the syringe needle. Connect the positive electrode of the high-voltage power supply to the syringe needle, and the negative electrode to the receiving roller. Set the spinning voltage to 15 kV, the solution propulsion speed to 0.5 mL / h, and the steel roller rotation speed to 120 rad / min. After electrospinning, a nanofilm material is obtained;

[0037] (3) Pre-oxidation: First, put the nanofilm material into an air circulation oven, set the temperature to 60°C, and set the time to 3 hours for preliminary oxidation, and the material will appear light yellow. Then set the temperature of the air circulation oven to 200°C and set the time to 2 hours for further oxidation, and the material will appear khaki. Finally, wait for the material to cool down naturally to complete the pre-oxidation;

[0038] (4) Carbonization: The material was placed in a tubular furnace and nitrogen was continuously introduced into the furnace. The temperature was increased linearly from room temperature at 5°C / min. When the temperature was increased to 1050°C and maintained for 1 h, the material gradually changed from khaki to black, completing the carbonization transformation process. The nitrogen was then introduced to room temperature to obtain a flexible ammonia-sensitive material, CNF / Al2O3.

[0039] Material characterization of Example 1:

[0040] The experimental instruments are scanning electron microscope (SEM) and its matching EDS spectrum, model Shimadzux-550, produced in Shimadzu, Japan. The CNF / Al2O3 material was observed by scanning electron microscope. The average diameter of the material fiber at 5μm magnification was 460nm, which was relatively uniform. The surface element distribution of CNF / Al2O3 material was characterized by EDS spectrum, mainly C, O and Al elements;

[0041] The Raman spectroscopy test instrument model is Jobin-Yvon Horiba T64000 Raman triple grating spectrum, the light source wavelength is 532nm, and the Raman test of CNF / Al2O3 material is carried out. D / I G The value of is 1.22, indicating that the material has more defects in the C atom lattice;

[0042] The experimental instrument is an X-ray photoelectron spectrometer (XPS) model Nexsa XPS, X-ray photoelectron spectroscopy (XPS) test and characterization of CNF / Al2O3 materials; carbon-containing functional groups mainly include CC (284.8eV), CO (286.67eV) and C=O (288.61eV), and the corresponding contents are 69.72at%, 18.7at% and 11.5at% respectively; O element mainly exists in three forms of Al2O3 (531.3eV), C=O (532.61eV) and CO (533.92eV), among which the Al2O3 content is 17.47at%, the C=O functional group content is 72.59at%, and the CO functional group content is 9.94at%; Al element has two material signal peaks, Al4C3 (73.13eV) and Al2O3 (74.18eV), and the corresponding contents are 35.55at% and 64.45at% respectively.

[0043] Example 2

[0044] (1) Solution preparation: Weigh 1.2 g of polyacrylonitrile powder (PAN) and add it to 8.8 g of N,N-dimethylformamide (DMF), and stir it in a water bath magnetic stirrer at 60°C and 150 r / min for 4 h until a uniform precursor solution is obtained. Then add 0.15 g of AlCl3 and 0.15 g of CaCl2, and stir it in a water bath magnetic stirrer at 60°C and 150 r / min for 6 h. After stirring evenly, let it stand for 24 h to degas, and obtain a spinning solution;

[0045] (2) Electrospinning: At a temperature of 20°C and a relative humidity of 40%, add the spinning solution into a syringe, and place the receiving roller 180 mm away from the syringe needle. Connect the positive electrode of the high-voltage power supply to the syringe needle, and the negative electrode to the receiving roller. Set the spinning voltage to 15 kV, the solution propulsion speed to 0.5 mL / h, and the steel roller rotation speed to 120 rad / min. After electrospinning, a nanofilm material is obtained;

[0046] (3) Pre-oxidation: First, put the nanofilm material into an air circulation oven, set the temperature to 60°C, and set the time to 3 hours for preliminary oxidation, and the material will appear light yellow. Then set the temperature of the air circulation oven to 200°C and set the time to 2 hours for further oxidation, and the material will appear khaki. Finally, wait for the material to cool down naturally to complete the pre-oxidation;

[0047] (4) Carbonization: The material was placed in a tubular furnace and nitrogen was continuously introduced into the furnace. The temperature was increased linearly from room temperature at 5°C / min. When the temperature was increased to 1050°C and maintained for 1 h, the nanofibers gradually changed from khaki to black, completing the carbonization transformation process. The nitrogen was then introduced to room temperature to obtain a flexible ammonia-sensitive material, Ca-doped CNF / Al2O3.

[0048] Material characterization was performed on Example 2:

[0049] The experimental instruments are scanning electron microscope (SEM) and its matching EDS spectrum, model Shimadzux-550, produced in Shimadzu, Japan. The Ca-doped CNF / Al2O3 material was observed by scanning electron microscope. The average fiber diameter was 390nm, the fiber diameter was highly uniform, and the surface was relatively smooth. The surface element distribution of the Ca-doped CNF / Al2O3 material was characterized by EDS spectrum, which mainly contained C, O, Al and Ca elements;

[0050] The Raman spectroscopy test instrument model is Jobin-Yvon Horiba T64000 Raman triple grating spectrum, the light source wavelength is 532nm, and the Ca-doped CNF / Al2O3 material is tested by Raman. The ID / IG value is 1.51, indicating that the material has more defects in the C atom lattice. The defects in the C atom lattice may increase the surface active sites of the material, which can be used as the location for gas molecule adsorption. More active sites may mean higher gas adsorption capacity, thereby improving gas sensing performance;

[0051] The experimental instrument is an X-ray photoelectron spectrometer (XPS) model Nexsa XPS, and the Ca-doped CNF / Al2O3 material is tested and characterized by X-ray photoelectron spectroscopy (XPS); the carbon-containing functional groups mainly include CC (284.8eV, 68.54at%), CO (286.14eV, 24.09at%) and C=O (289.08eV, 7.37at%); the O element is mainly in the form of CaO (529.87eV), Al2O3 (531.25eV), C=O (532.53eV) and CO (533.82eV) exists in four forms, among which the CaO content is 5.58at%, the Al2O3 content is 44.84at%, the C=O functional group content is 40.33at%, and the CO functional group content is 9.25at%; the Al element has two material signal peaks, Al4C3 (73.1eV) and Al2O3 (74.37eV), and the corresponding contents are 40.64at% and 59.36at%, respectively; the Ca element has four signal peaks, CaC2 2p3 / 2 (346.8 2eV) and CaC2 2p 1 / 2 (eV), CaO 2p 3 / 2 (347.86 eV) and CaO 2p 1 / 2 (351.17eV), CaC2 content is 42.43at%, and CaO content is 57.57at%.

[0052] The present invention uses the two flexible ammonia sensitive materials to package electrodes and conducts tests in an ammonia environment;

[0053] The gas-sensitive test environment adopts a straight-through method, using a thickened and sealed component box, with an ambient temperature of 20-25°C and a humidity of 20%-30%. The flexible ammonia sensitive material is placed in the component box, and the test electrode is connected to the digital source meter. A mixing chamber is set at the inlet of the component box, and high-concentration test gas and nitrogen are filled into the mixing chamber at different flow rates, and then enter the component box. The outlet of the component box is connected to the exhaust gas treatment equipment. During the test, each concentration ratio is ventilated for about 10 minutes, and the input and output ports of the component box are closed to measure the change in the resistance of the material. The response value of Ca-doped CNF / Al2O3 flexible ammonia sensitive material is higher than that of CNF / Al2O3 flexible ammonia sensitive material.

[0054] The selectivity of Ca-doped CNF / Al2O3 flexible ammonia sensitive material was tested for ethanol, DMF, NH3, HCl and methanol. At room temperature, Ca-doped CNF / Al2O3 flexible ammonia sensitive material has ultra-high selectivity for NH3, while its sensitivity to other test gases is relatively low.

[0055] The response / recovery time test of the Ca-doped CNF / Al2O3 flexible ammonia sensitive material with a 0-50ppm ammonia concentration was carried out in a gas-sensitive test environment, and the test was repeated 5 times. The response / recovery time of the Ca-doped CNF / Al2O3 flexible ammonia sensitive material prepared by the present invention is 221s / 226s, and it still maintains good response and recovery capabilities after multiple cycle tests. The resistance peak value in the cycle test remains basically unchanged, and it has good sensing characteristics and repeatability.

[0056] In order to evaluate the long-term stability and service life of Ca-doped CNF / Al2O3 flexible ammonia sensitive materials, the gas-sensitive materials were placed in a gas-sensitive test device containing 50ppm ammonia for 15 days, and the resistance changes were recorded at fixed time points every day. The resistance of the material remained almost unchanged within 15 days, indicating that the material has good long-term stability.

[0057] The Ca-doped CNF / Al2O3 flexible ammonia sensitive material was placed in a humidity testing device for resistance collection, and the resistance values ​​at different humidity were recorded, with the humidity range of 20% to 80%; the Ca-doped CNF / Al2O3 flexible ammonia sensitive material was placed in a temperature testing device for resistance collection, and the resistance values ​​at different temperatures were recorded, with the temperature range of 20℃ to 60℃. The test showed that changes in temperature and humidity have little effect on the resistance change rate and do not have a good linear relationship, which proves that the prepared Ca-doped CNF / Al2O3 flexible ammonia sensitive material is insensitive to temperature and humidity and has good environmental stability.

[0058] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method for preparing a flexible ammonia sensitive material, characterized in that: The flexible ammonia sensitive material comprises the following preparation steps: (1) Solution preparation: Polyacrylonitrile (PAN) is dissolved in N,N-dimethylformamide (DMF) as a precursor solution, and an aluminum source and a calcium source are added thereto to obtain a spinning solution; (2) Preparation of flexible ammonia sensitive materials: Nano-thin film materials were prepared by electrospinning technology, and flexible ammonia sensitive materials—Ca-doped CNF / Al2O3—were obtained after pre-oxidation and carbonization.

2. The method for preparing a flexible ammonia sensitive material according to claim 1, characterized in that: In step (1), the molecular weight of polyacrylonitrile is 15,000, and the mass concentration of the precursor solution is 12%.

3. The method for preparing the flexible ammonia sensitive material according to claim 1, characterized in that: In step (1), the aluminum source is aluminum chloride (AlCl3) and the Ca source is calcium chloride (CaCl2).

4. The method for preparing a flexible ammonia sensitive material according to claim 1, characterized in that: The electrospinning process in step (2) is carried out at a temperature of 20° C., a relative humidity of 40%, a voltage of 15 kV, a receiving spacing of 180 mm, a solution advancing speed of 0.5 mL / h, and a roller speed of 120 rad / min for 2 hours to obtain a nano film material.

5. The method for preparing a flexible ammonia sensitive material according to claim 1, characterized in that: In step (2), the pre-oxidation first places the nanofilm material into an air circulation oven, sets the temperature to 60°C, and the time to 3 hours for preliminary oxidation, then sets the temperature of the air circulation oven to 200°C and the time to 2 hours for further oxidation, and finally waits for the material to cool down naturally to complete the pre-oxidation.

6. The method for preparing a flexible ammonia sensitive material according to claim 1, characterized in that: In step (2), the carbonization material is placed in a tubular furnace, and nitrogen is continuously filled into the tubular furnace. The temperature is steadily increased linearly from room temperature at 5°C / min. When it is increased to 1050°C and maintained for 1h, the carbonization process is completed to obtain a flexible ammonia sensitive material - Ca-doped CNF / Al2O3.