Method for recovering aluminum phosphate from sludge

By leaching organic acid and hydrothermal synthesis of sludge incineration ash, industrial-grade aluminum phosphate is directly obtained, which solves the problem of long process flow in the existing technology, improves production efficiency and product purity, and achieves high efficiency of sludge resources use.

CN119079953AActive Publication Date: 2024-12-06HUAZHONG UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411205071.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

In the prior art, the process flow of recovering aluminum phosphate from sludge is relatively long, resulting in low production efficiency and high cost.

Method used

By incinerating the dried sludge, leaching the sludge incineration ash with the target organic acid at a preset concentration, hydrothermal synthesis is carried out after solid-liquid separation, industrial-grade aluminum phosphate is directly obtained, simplifying the process flow and saving The cost.

Benefits of technology

The process flow for preparing industrial grade aluminum phosphate is shortened, the leaching rate and purity of aluminum phosphate is improved, the process cost is reduced, and the efficient utilization of sludge resources is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079953A_ABST
    Figure CN119079953A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sludge resource utilization, in particular to a method for recycling aluminum phosphate from sludge. According to the technical scheme, dried sludge is incinerated to obtain sludge incineration ash, then the sludge incineration ash is leached through target organic acid with the preset concentration, phosphorus-containing leachate is obtained after solid-liquid separation, the phosphorus-containing leachate is subjected to hydrothermal synthesis, and the industrial-grade aluminum phosphate is obtained. Therefore, according to the technical scheme, the phosphorus-containing leachate obtained after the target organic acid with the preset concentration is leached is directly subjected to hydro-thermal synthesis treatment, and therefore the technological process for preparing the industrial-grade aluminum phosphate can be shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sludge resource utilization, and in particular to a method for recovering aluminum phosphate from sludge. Background Art

[0002] Pollutants and nutrients in sewage are aggregated by the massive growth of bacteria and chemical agents, eventually forming sludge. With the rapid development of industries such as functional materials, refractory materials, ceramics and new molecular sieves, the output of industrial-grade aluminum phosphate is also rising, resulting in an increase in the demand for its production raw materials (such as phosphorus).

[0003] In the related art, the method for recovering phosphorus from sludge and preparing industrial-grade aluminum phosphate mainly adopts wet chemical method, but the process flow of this method is relatively long.

[0004] Therefore, there is an urgent need for a method for recovering aluminum phosphate from sludge to solve this technical problem. Summary of the invention

[0005] The invention provides a method for recovering aluminum phosphate from sludge, which can shorten the process flow of preparing industrial-grade aluminum phosphate.

[0006] The present invention provides a method for recovering aluminum phosphate from sludge, comprising:

[0007] Incinerating the dried sludge to obtain sludge incineration ash;

[0008] Leaching the sludge incineration ash with a target organic acid of a preset concentration, and obtaining a phosphorus-containing leaching solution after solid-liquid separation;

[0009] The phosphorus-containing leaching solution is subjected to hydrothermal synthesis to obtain industrial-grade aluminum phosphate.

[0010] As can be seen from the above scheme, the present invention provides a method for recovering aluminum phosphate from sludge, by incinerating the dried sludge to obtain sludge incineration ash, then leaching the sludge incineration ash with a target organic acid of a preset concentration, and obtaining a phosphorus-containing leachate after solid-liquid separation, and hydrothermally synthesizing the phosphorus-containing leachate to obtain industrial-grade aluminum phosphate. Therefore, the above technical scheme is to directly perform hydrothermal synthesis treatment on the phosphorus-containing leachate after leaching with a target organic acid of a preset concentration, so that the process flow of preparing industrial-grade aluminum phosphate can be shortened. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0012] Figure 1 A schematic diagram of a method for recovering aluminum phosphate from sludge provided in an embodiment of the present invention;

[0013] Figure 2 A comparison chart of aluminum phosphate recovered by the method provided in the embodiment of the present invention and commercial grade aluminum phosphate;

[0014] Figure 3 A thermodynamic equilibrium calculation system diagram of the precipitation reaction between impurity components in the phosphorus-containing leachate and the target phosphorus-containing product provided in an embodiment of the present invention;

[0015] Figure 4 A Gibbs free energy change diagram of the aluminum phosphate precipitation reaction provided in an embodiment of the present invention;

[0016] Figure 5 A reaction equilibrium constant diagram for the aluminum phosphate precipitation reaction provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0018] See also Figure 1 One embodiment of the present invention provides a method for recovering aluminum phosphate from sludge, the method comprising:

[0019] Step 100, incinerating the dried sludge to obtain sludge incineration ash;

[0020] Step 102: leaching the sludge incineration ash with a target organic acid of a preset concentration, and obtaining a phosphorus-containing leaching solution after solid-liquid separation;

[0021] Step 104: Perform hydrothermal synthesis on the phosphorus-containing leaching solution to obtain industrial-grade aluminum phosphate.

[0022] In this embodiment, the dried sludge is incinerated to obtain sludge incineration ash, and then the sludge incineration ash is leached with a target organic acid of a preset concentration, and a phosphorus-containing leachate is obtained after solid-liquid separation, and the phosphorus-containing leachate is hydrothermally synthesized to obtain industrial-grade aluminum phosphate. Therefore, the above technical scheme is to directly perform hydrothermal synthesis on the phosphorus-containing leachate after leaching with a target organic acid of a preset concentration, so that the process flow of preparing industrial-grade aluminum phosphate can be shortened.

[0023] In some embodiments, the incineration temperature is 750-900° C. to ensure the incineration effect of the dried sludge.

[0024] In one embodiment of the present invention, the target organic acid includes at least one of oxalic acid, citric acid, acetic acid and ascorbic acid.

[0025] In this embodiment, the sludge will accumulate a large amount of aluminum from the external environment during its formation, resulting in the molar amount of aluminum in the sludge itself being often greater than the molar amount of phosphorus. This means that if the aluminum and phosphorus in the sludge can be leached out simultaneously, there is no need to add an aluminum source from the outside in the subsequent precipitation process, and this method saves process expenses. In order to achieve the above purpose, the type and concentration of the target organic acid are optimized, and it is determined that the target organic acid is used to leach the sludge incineration ash. These target organic acids can achieve complete leaching of phosphorus through their own strong acidity, reducibility and the chelating properties of acid radicals, while ensuring that enough aluminum enters the phosphorus-containing leachate simultaneously, and utilizes the organic acid radicals in the target organic acid and the aluminum phosphate in the sludge incineration ash to undergo precipitation reaction, and at the same time, the above target organic acid can be destroyed in a hydrothermal environment, thereby achieving the synchronous precipitation of aluminum and phosphorus.

[0026] In the related art, some leachates are usually added with metal source reagents in corresponding molar ratios. However, the price of Al salts represented by AlCl3 is as high as 7,000 yuan / ton, which greatly increases the process cost of the recovery process, and the process is complicated and lengthy. During leaching, Fe, Ca, Mg and other elements in the sludge will be leached synchronously with the P element. In order to avoid the formation of impurities, it is often necessary to remove impurities by adjusting the pH pre-precipitation method, cation exchange resin method, etc. The pH is then adjusted to the most suitable precipitation range for the target product to obtain the highest possible yield. However, the target organic acid in this embodiment can achieve the simultaneous leaching of phosphorus and aluminum elements in sludge incineration ash without the addition of an external Al source, pH adjustment, and filtrate purification. Such a method effectively simplifies the treatment process and reduces the treatment cost.

[0027] In one embodiment of the present invention, the preset concentration is 0.04-0.15 mol / L, at which the leaching effect of the target organic acid on phosphorus in the sludge incineration ash can be guaranteed.

[0028] In one embodiment of the present invention, the solid-liquid ratio of sludge incineration ash to target organic acid is 1:50-1:200, the leaching time is 2-4 hours, and the tumbling oscillation rate is 60-200 rpm to ensure the leaching effect of the target organic acid on the phosphorus element in the sludge incineration ash.

[0029] In one embodiment of the present invention, the pH value of the phosphorus-containing leaching solution is 1-2.

[0030] In this embodiment, by adding the target organic acid to adjust the pH value of the phosphorus-containing leaching solution to 1-2, it can help to recover aluminum phosphate from the sludge incineration ash at room temperature, and at the same time ensure that the phosphorus leaching rate of the sludge incineration ash can reach more than 90%, and the aluminum leaching rate can reach more than 70%.

[0031] Thermodynamic calculations show that under hydrothermal reaction conditions, AlPO4 has an independent precipitation interval under the acidic conditions of strong target organic acids with a pH of 1 to 2, such as Figure 3 As shown in the figure (the width of the horizontal bar of each substance represents the degree of precipitation reaction under the corresponding pH conditions), other phosphorus-containing products (such as Fe3(PO4)2, MgNH4PO4, Ca5(PO4)3OH) and solid impurities (such as Fe(OH)3, Al(OH)3, Mg(OH)2, CaC2O4) cannot undergo precipitation reaction in this range. Therefore, it is only necessary to control the target organic acid concentration and ensure that the pH value of the phosphorus-containing leachate is within this range to achieve the separate precipitation of AlPO4, and at the same time, the purity of the phosphorus-containing leachate can be guaranteed.

[0032] In some embodiments, the phosphorus-containing leachate after leaching can be filtered using a filter head of, for example, 0.45 μm, to remove the solid particles that have not been separated cleanly in the phosphorus-containing leachate.

[0033] In one embodiment of the present invention, the phosphorus-containing leaching solution is used for cyclic leaching of new sludge incineration ash.

[0034] In this embodiment, the phosphorus-containing leachate is recycled to the cyclic leaching of phosphorus in the sludge incineration ash, which can reduce reagent consumption.

[0035] In one embodiment of the present invention, when the pH value of the phosphorus-containing leachate is greater than 2, the circulation leaching of the phosphorus-containing leachate is stopped.

[0036] In this embodiment, if the pH value of the phosphorus-containing leachate is greater than 2, the separate precipitation of AlPO4 cannot be guaranteed, and the purity of the phosphorus-containing leachate is affected. When the pH value of the phosphorus-containing leachate is less than 2 and greater than 1, the phosphorus-containing leachate can be used for circulating leaching of new sludge incineration ash.

[0037] In one embodiment of the present invention, the molar ratio of aluminum element to phosphorus element in the phosphorus-containing leachate is greater than 1:1.

[0038] In some embodiments, if the molar ratio of aluminum to phosphorus in the phosphorus-containing leachate is less than 1:1, additional AlCl3 is added to make the molar ratio of aluminum to phosphorus in the phosphorus-containing leachate reach 1:1. At this time, the additional aluminum source required is generally less than 20% of the total aluminum source required for preparing industrial-grade aluminum phosphate.

[0039] In one embodiment of the present invention, the reaction temperature of the hydrothermal synthesis is 150-210° C., and the reaction time is 2-24 hours to ensure that the phosphorus-containing leachate reacts fully.

[0040] In one embodiment of the present invention, step 104 may specifically include:

[0041] Performing hydrothermal synthesis on the phosphorus-containing leaching solution to obtain a hydrothermal synthesis product;

[0042] Performing solid-liquid separation on the hydrothermal synthesis product to obtain a solid product;

[0043] The solid product is washed a preset number of times with a deionized water mixed solution, and the washed solid product is freeze-dried to obtain industrial-grade aluminum phosphate.

[0044] In this embodiment, under the heating condition of the target organic acid with a preset concentration, the precipitation reaction of the relevant impurities and other phosphorus-containing products except AlPO4 can be further suppressed. In the phosphorus-containing leachate, Al ions exist in the form of Al-acid ligands (taking the oxalic acid system as an example, Al exists in the form of Al(C2O4)3 3- This coordination compound exists) without combining with phosphorus. Under the hydrothermal environment, the organic acid radical decomposes, making Al 3+ is released again and can react with PO4 3- A precipitation reaction occurs to generate AlPO4. The precipitation reaction of AlPO4 is a reversible reaction at low temperature (equilibrium constant lgK<5), which will result in low yield of AlPO4 and slow synthesis rate. However, the hydrothermal method can achieve a reaction equilibrium constant lgK>5 at above 150°C, making the synthesis reaction more thorough and faster. Figure 4 (When △G < 0, the reaction is considered to be spontaneous) and Figure 5 (When lgK>5, the precipitation reaction is considered to be more complete).

[0045] The aluminum phosphate produced by hydrothermal treatment presents a uniform microcrystalline particle structure, and the products are all flower-shaped microcrystalline particles with high crystallinity at the microscopic level. The Al, P and O elements present a uniform symbiotic distribution, such as Figure 2As shown, aluminum phosphate has better microstructure and product performance.

[0046] exist Figure 2 In the figure, a and b are respectively the macroscopic morphology comparisons of the aluminum phosphate obtained by the method and commercial grade aluminum phosphate, c and d are respectively the microscopic morphology comparisons of the aluminum phosphate obtained by the method and commercial grade aluminum phosphate, e is the element distribution uniformity test of the aluminum phosphate obtained by the method and the crystal structure comparison of commercial grade aluminum phosphate, and f is the crystal structure comparison of the aluminum phosphate recovered by the method and commercial grade aluminum phosphate. Figure 2 It can be seen that the aluminum phosphate prepared in the embodiment of the present invention has greatly improved uniformity.

[0047] In an embodiment of the present invention, the impurity content of aluminum phosphate can reach the standard of TZJCX0002-2022 industrial aluminum phosphate and analytical pure reagents, and the data are shown in Table 1 (showing the content of industrial grade aluminum phosphate, analytical pure reagent grade and recovered product of this method).

[0048] Table 1 Comparison of aluminum phosphate and standard limits

[0049]

[0050] In this embodiment, vacuum filtration is used to separate the hydrothermal synthesis product into solid and liquid, so that the hydrothermal synthesis product can be better separated into solid and liquid.

[0051] In this embodiment, deionized water is used for washing to remove impurity ions in the solid product.

[0052] In this embodiment, the washed solid product is freeze-dried to remove moisture from the solid product and obtain industrial-grade aluminum phosphate.

[0053] In some embodiments, the phosphorus-containing leachate is directly placed in a closed container for hydrothermal reaction, and stirring is not required during the reaction process.

[0054] Through the above method, a large number of calculations and experiments are carried out on the ion thermodynamic reaction equilibrium system in the phosphorus-containing leachate. By selecting the type and concentration of the target organic acid, the sludge incineration ash is leached so that the phosphorus and aluminum in the sludge incineration ash are leached synchronously, so that the phosphorus-containing leachate after leaching reaches the hydrothermal condition, and the phosphorus-containing leachate is hydrothermally synthesized, so that aluminum phosphate is directly synthesized using only the aluminum element inside the sludge incineration ash. This method does not require the addition of an external aluminum source, saving the cost of reagents, and does not require the removal of impurities by adjusting the pH and purifying the filtrate, shortening the process of recovering phosphorus from sludge and preparing industrial-grade aluminum phosphate. This method not only realizes the resource utilization of sludge, but also achieves the purpose of preparing industrial-grade aluminum phosphate.

[0055] The above specific embodiments further illustrate the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recovering aluminum phosphate from sludge, characterized in that: include: Incinerating the dried sludge to obtain sludge incineration ash; Leaching the sludge incineration ash with a target organic acid of a preset concentration, and obtaining a phosphorus-containing leaching solution after solid-liquid separation; The phosphorus-containing leaching solution is subjected to hydrothermal synthesis to obtain industrial-grade aluminum phosphate.

2. The method according to claim 1, characterized in that: The target organic acid includes at least one of oxalic acid, citric acid, acetic acid and ascorbic acid.

3. The method according to claim 1, characterized in that The preset concentration is 0.04-0.15 mol / L.

4. The method according to claim 1, characterized in that: The solid-liquid ratio of the sludge incineration ash to the target organic acid is 1:50-1:200, the leaching time is 2-4 hours, and the tumbling oscillation rate is 60-200 rpm.

5. The method according to claim 1, characterized in that The pH value of the phosphorus-containing leaching solution is 1-2.

6. The method according to claim 5, characterized in that The phosphorus-containing leaching solution is used for cyclic leaching of new sludge incineration ash.

7. The method according to claim 6, characterized in that When the pH value of the phosphorus-containing leaching solution is greater than 2, the circulation leaching of the phosphorus-containing leaching solution is stopped.

8. The method according to claim 1, characterized in that The molar ratio of aluminum element to phosphorus element in the phosphorus-containing leaching solution is greater than 1:

1.

9. The method according to claim 1, characterized in that: The reaction temperature of the hydrothermal synthesis is 150-210° C., and the reaction time is 2-24 hours.

10. The method according to any one of claims 1 to 9, characterized in that The step of subjecting the mixed solution to hydrothermal synthesis to obtain industrial-grade aluminum phosphate comprises: Performing hydrothermal synthesis on the phosphorus-containing leachate to obtain a hydrothermal synthesis product; Performing solid-liquid separation on the hydrothermal synthesis product to obtain a solid product; The solid product is washed a preset number of times with a deionized water mixed solution, and the washed solid product is freeze-dried to obtain industrial-grade aluminum phosphate.

Citation Information

Patent Citations

  • Method for combined treatment of converter slag and sludge incineration ash and phosphorus recovery

    CN117623248A

  • Resource recovery method for material essentially consisting of aluminum phosphate

    JP2002018399A