Preparation method and application of manganese phosphate
By preparing manganese phosphate under normal pressure, the reaction of manganese source, oxidant and alkali is used to generate MnPO4·H2O, which solves the problems of low yield and high cost of preparation of lithium manganese phosphate in the prior art, and achieves high efficiency and low Cost preparation of manganese phosphate and good electrochemical properties.
Patent Information
- Application Number
- CN202411426433.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
AI Technical Summary
In the existing preparation methods for lithium manganese phosphate, the reaction temperature of manganese hydrogen phosphate is high, the reaction time is long, the yield is low, and the use of soluble divalent manganese salts and excessive phosphoric acid produces a large amount of acid-containing wastewater, which increases production costs and limits large-scale Feasibility of production.
By using the manganese phosphate preparation method under normal pressure, the first reaction of a mixed solution containing a manganese source, an oxidant and a alkali is carried out to generate MnO(OH), and then the second reaction is carried out to generate MnPO4·H2O. The whole process is operated Simple, low production cost, and yield is close to 100%.
The high yield and low cost preparation of manganese phosphate are achieved, avoiding the problem of low yields of Mn and P. The prepared manganese phosphate has good quality, is suitable for large-scale industrial production, and is used to prepare phosphoric acid with good electrochemical properties. Lithium material.
Smart Images

Figure CN119079959A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery material synthesis, and in particular to a method for preparing manganese phosphate and application thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, long service life, and good safety. They have been widely used in consumer electronics, electric vehicles, large-scale energy storage and other fields, greatly improving the lives of modern people. As a lithium-ion battery positive electrode material, lithium manganese phosphate has a discharge platform of up to 4.1V, and its theoretical energy density is 20% higher than that of lithium iron phosphate. Its stable PO bond and olivine structure give it good thermal stability and high safety performance. In addition, its charge and discharge voltage is compatible with the electrochemical window of existing commercial electrolytes. Therefore, lithium manganese phosphate is considered to be the next generation of positive electrode materials that are expected to replace lithium iron phosphate and achieve commercial application.
[0003] At present, the methods for preparing lithium manganese phosphate mainly include high temperature solid phase method, hydrothermal method, coprecipitation method and mechanical ball milling method. Among them, the high temperature solid phase method mostly uses the mixing of manganese source, phosphorus source, lithium source and carbon source, and then goes through the processes of sand milling, spray drying and sintering. It has low equipment requirements and is easy to operate, which is most suitable for industrial production.
[0004] Patent CN101673821A discloses a method for preparing lithium manganese phosphate / carbon composite material with manganese hydrogen phosphate, first hydrothermally reacting a soluble divalent manganese salt with excess phosphoric acid to obtain manganese hydrogen phosphate, and then milling it with a lithium source and a carbon source, spray drying and calcining to prepare lithium manganese phosphate. However, in the above-mentioned preparation method, the reaction temperature of manganese hydrogen phosphate is high and the reaction time is long, the yield is low, and a soluble divalent manganese salt and excess phosphoric acid are used at the same time, a large amount of acid-containing wastewater is produced, which greatly increases the production cost and is not conducive to large-scale production. Therefore, it is necessary to develop a preparation method of manganese phosphate, a precursor of lithium manganese phosphate, which is simple to operate, low in cost, and suitable for large-scale production.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] In view of the above-mentioned defects in the prior art, the present invention provides a method for preparing manganese phosphate and its application. The method for preparing manganese phosphate is simple to operate, does not rely on complex process equipment, has low production cost and high yield, and the prepared manganese phosphate has good quality.
[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0008] One aspect of the present invention relates to a method for preparing manganese phosphate, comprising the following steps:
[0009] (a) subjecting a mixed solution containing a manganese source, an oxidant and an alkali to a first reaction to obtain MnO(OH);
[0010] (b) The mixed solution containing MnO(OH) and H3PO4 is subjected to a second reaction to obtain MnPO4·H2O.
[0011] The method for preparing manganese phosphate can be completed under normal pressure conditions. The entire preparation process is simple to operate, has low production cost, and a yield of nearly 100%. The problem of low Mn and P yields caused by the generation of MnHPO4·3H2O can be avoided, and the prepared manganese phosphate has good quality.
[0012] Preferably, the Mn in the manganese source is 2+ The molar ratio of the oxidant to the oxidant is 1:0.7-0.8.
[0013] Preferably, the pH of the first reaction is 7.0-9.5.
[0014] Preferably, the first reaction time is 2 to 3 hours.
[0015] Preferably, the pH of the second reaction is 1.6-2.0.
[0016] Preferably, the second reaction time is 2 to 3 hours.
[0017] Preferably, the manganese source includes: a divalent manganese salt.
[0018] Preferably, the divalent manganese salt comprises at least one of MnSO4, MnCl2, Mn(NO3)2 or Mn(CH3COO)2.
[0019] Preferably, the oxidant comprises at least one of H2O2, NaClO or HClO.
[0020] Preferably, the base comprises at least one of NaOH, KOH or ammonia water.
[0021] Another aspect of the present invention also relates to a method for preparing lithium manganese phosphate, wherein MnPO4·H2O prepared by the method for preparing manganese phosphate, a lithium source and a carbon source are ball-milled, spray-dried and calcined to obtain LiMnPO4.
[0022] Another aspect of the present invention also relates to a secondary battery, in which the lithium manganese phosphate prepared by the lithium manganese phosphate preparation method is used as a positive electrode material.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The method for preparing manganese phosphate provided by the present invention comprises: 2+As a manganese source, Mn 2+ Oxidized to Mn 3+ The compound MnO(OH) is reacted with H3PO4 to obtain MnPO4·H2O with a yield close to 100%, which can avoid the problem of low Mn and P yields caused by the generation of MnHPO4·3H2O. The prepared manganese phosphate has good quality, and the manganese lithium phosphate prepared using it has good electrochemical properties.
[0025] (2) The method for preparing manganese phosphate provided by the present invention can be completed under normal pressure conditions. The entire preparation process is simple to operate and can greatly reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The XRD pattern of MnPO4·H2O prepared in the embodiment of the present invention;
[0028] Figure 2 This is the XRD spectrum of LiMnPO4 prepared in the embodiment of the present invention. DETAILED DESCRIPTION
[0029] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If the specific conditions are not indicated in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0030] One aspect of the present invention relates to a method for preparing manganese phosphate, comprising the following steps:
[0031] (a) subjecting a mixed solution containing a manganese source, an oxidant and an alkali to a first reaction to obtain MnO(OH);
[0032] (b) The mixed solution containing MnO(OH) and H3PO4 is subjected to a second reaction to obtain MnPO4·H2O.
[0033] The method for preparing manganese phosphate comprises using divalent manganese salt as a manganese source, reacting Mn with an oxidant under alkaline conditions. 2+ Oxidized to Mn 3+ The compound MnO(OH) is then reacted with phosphoric acid (H3PO4) to obtain manganese phosphate (MnPO4·H2O). The entire preparation process is simple to operate, and the yield of MnPO4·H2O is close to 100%, which is very suitable for large-scale industrial production. The prepared MnPO4·H2O precursor can be mixed with a lithium source and a carbon source, ball milled, spray dried, and calcined to prepare lithium manganese phosphate (LiMnPO4). The prepared lithium manganese phosphate has good electrochemical properties.
[0034] Furthermore, the manganese source includes: divalent manganese salt.
[0035] The present invention does not specifically limit the specific type of divalent manganese salt, and conventional existing divalent manganese salts in the art can be used to implement the technical solution of the present invention. In some specific embodiments, the divalent manganese salt includes but is not limited to at least one of MnSO4·H2O, MnCl2·4H2O, Mn(NO3)2·4H2O or Mn(CH3COO)2·4H2O.
[0036] Furthermore, the divalent manganese salt is added in the form of a solution, wherein Mn 2+ The concentration is 60-90 g / L, including but not limited to any one of 60 g / L, 65 g / L, 70 g / L, 75 g / L, 80 g / L, 85 g / L or 90 g / L or the range between any two of them.
[0037] Furthermore, the divalent manganese salt solution is stirred in a magnetic heating stirrer, and the magnetic heating temperature is 60-90°C, including but not limited to any point value of 60°C, 70°C, 80°C or 90°C or a range value between any two of them.
[0038] Furthermore, the oxidant includes but is not limited to at least one of H2O2, NaClO or HClO.
[0039] Furthermore, the base includes but is not limited to: at least one of NaOH, KOH or ammonia water.
[0040] Furthermore, the Mn in the manganese source 2+ The molar ratio of Mn to the oxidant is 1:0.7 to 0.8, including but not limited to 1:0.7, 1:0.75 or 1:0.8. 2+ The molar ratio of the oxidant to the Mn 2 + Oxidized to Mn 3+, which is beneficial to the reaction and can also avoid waste caused by excessive oxidant.
[0041] Furthermore, the pH of the first reaction is 7.0 to 9.5, including but not limited to any point value of 7.0, 7.5, 8.0, 8.5, 9.0 or 9.5 or any range value between two of them. Controlling the pH of the first reaction within a reasonable range can ensure that Mn 2+ Under alkaline conditions, it is completely oxidized to form Mn 3+ Compound MnO(OH).
[0042] Furthermore, the time of the first reaction is 2 to 3 hours, including but not limited to any one of 2 hours, 2.4 hours, 2.8 hours or 3 hours or any range between two of them. Controlling the time of the first reaction within a reasonable range can ensure that the reaction is fully carried out and the target product is obtained.
[0043] Furthermore, the pH of the second reaction is 1.6 to 2.0, including but not limited to any point value of 1.6, 1.7, 1.8, 1.9 or 2.0 or a range of values between any two of them. Controlling the pH of the second reaction within a reasonable range can ensure that MnO(OH) and H3PO4 fully react to generate MnPO4·H2O.
[0044] Furthermore, the time of the second reaction is 2 to 3 hours, including but not limited to any one of 2 hours, 2.4 hours, 2.8 hours or 3 hours or any range between two of them. Controlling the time of the second reaction within a reasonable range can ensure that the reaction is fully carried out and the target product is harvested.
[0045] Furthermore, the MnO(OH) participates in the second reaction in the form of slurry, and the solid content of the MnO(OH) slurry is 10% to 20%.
[0046] Furthermore, the MnO(OH) slurry is stirred in a magnetic heating stirrer, and the magnetic heating temperature is 60-90°C, including but not limited to any point value of 60°C, 70°C, 80°C or 90°C or a range value between any two of them.
[0047] Another aspect of the present invention also relates to a method for preparing lithium manganese phosphate, wherein the manganese phosphate, a lithium source and a carbon source prepared by the method for preparing manganese phosphate are ball-milled, spray-dried and calcined to obtain the lithium manganese phosphate.
[0048] The lithium manganese phosphate prepared by the lithium manganese phosphate preparation method has excellent electrochemical properties.
[0049] Furthermore, the molar ratio of the lithium source to the MnPO4·H2O is 1:1.00 to 1.02, including but not limited to 1:1.00, 1:1.01 or 1:1.02.
[0050] Furthermore, the molar ratio of the carbon source to the MnPO4·H2O is 1:0.06-0.08, including but not limited to 1:0.06, 1:0.07 or 1:0.08.
[0051] Furthermore, the rotation speed of the ball mill is 300-600 r / min, including but not limited to any point value of 300 r / min, 350 r / min, 400 r / min, 450 r / min, 500 r / min, 550 r / min or 600 r / min or any range value between two thereof. Controlling the rotation speed of the ball mill within a reasonable range can ensure that MnPO4·H2O, lithium source and carbon source are fully mixed, while effectively controlling the slurry particle size.
[0052] Furthermore, the ball milling time is 6 to 12 hours, including but not limited to any one of 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours or 12 hours or a range between any two of them.
[0053] Furthermore, the calcination is carried out under a protective gas, and the protective gas includes but is not limited to at least one of N2, Ar or H2.
[0054] Furthermore, the calcination temperature is 700-850° C., including but not limited to any point value of 700° C., 720° C., 740° C., 760° C., 780° C., 800° C., 830° C. or 850° C. or a range value between any two of them. Controlling the calcination temperature within a reasonable range can ensure that MnPO4·H2O fully reacts with the lithium source and the carbon source to generate LiMnPO4, while effectively controlling the particle size.
[0055] Furthermore, the calcination time is 8 to 12 hours, including but not limited to any one of 8 hours, 9 hours, 10 hours, 11 hours or 12 hours or a range between any two of them.
[0056] The present invention does not specifically limit the specific type of lithium source, and any conventional lithium source in the art can be used to implement the technical solution of the present invention. In some specific embodiments, the lithium source includes but is not limited to at least one of lithium carbonate, lithium hydroxide, lithium oxalate or lithium acetate.
[0057] The present invention does not specifically limit the specific type of carbon source, and conventional carbon sources in the art can be used to implement the technical solution of the present invention. In some specific embodiments, the carbon source includes at least one of sucrose, glucose, fructose or starch.
[0058] Another aspect of the present invention also relates to a secondary battery, in which the lithium manganese phosphate prepared by the lithium manganese phosphate preparation method is used as a positive electrode material.
[0059] The reaction equation involved in the present invention is as follows:
[0060] Mn 2+ +H2O2+OH - →MnO(OH)+H2O;
[0061] Mn 2+ +ClO - +OH - →MnO(OH)+Cl - +H2O;
[0062] MnO(OH)+H3PO4→MnPO4·H2O+H2O;
[0063] MnPO4·H2O+Li2CO3+C 12 H 22 O 11 →LiMnPO4 / C+CO2+H2O.
[0064] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0065] Example 1
[0066] The method for preparing manganese phosphate provided in this embodiment comprises the following steps:
[0067] Step S1: 50.70 g MnSO4·H2O was dissolved in 275 mL deionized water to prepare Mn 2+ The solution was 60 g / L and stirred in a magnetic heating stirrer at 60 °C;
[0068] Step S2: Press n(Mn 2+ ):n(H2O2) molar ratio is 1:0.75. Weigh H2O2, add it and NaOH to MnSO4 solution at the same time and adjust the pH to 9.50. After reacting for 2 hours, filter and wash to obtain MnO(OH) filter cake;
[0069] Step S3: Take an appropriate amount of MnO(OH) filter cake, prepare it into a slurry with a solid content of 15%, place it in a 60°C magnetic heating stirrer and stir, add H3PO4 to adjust the solution pH to 1.6, react for 2 hours, filter, wash and dry to obtain MnPO4·H2O powder.
[0070] Figure 1 The XRD spectrum of MnPO4·H2O prepared by the above method is shown in Figure 2. From the results, it can be seen that the diffraction peaks of the product correspond to the standard diffraction peaks of monoclinic MnPO4·H2O (PDF#44-0071), there is no impurity peak, the peak intensity is high and the peak shape is sharp, indicating that pure phase MnPO4·H2O with good crystallinity is prepared by the above method.
[0071] Example 2
[0072] The method for preparing manganese phosphate provided in this embodiment comprises the following steps:
[0073] Step S1: MnCl2·4H2O is dissolved in 275 mL of deionized water to prepare Mn 2+ The solution was 60 g / L and stirred in a magnetic heating stirrer at 60 °C;
[0074] Step S2: Press n(Mn 2+ ):n(NaClO) molar ratio is 1:0.7. Weigh NaClO, add it and NaOH to MnCl2 solution at the same time and adjust the pH to 7.0. After reacting for 2.5 hours, filter and wash to obtain MnO(OH) filter cake;
[0075] Step S3: Take an appropriate amount of MnO(OH) filter cake and prepare it into a slurry with a solid content of 15%, place it in a 60°C magnetic heating stirrer and stir, add H3PO4 to adjust the solution pH to 1.8, react for 2.5 hours, filter, wash and dry to obtain MnPO4·H2O powder.
[0076] Example 3
[0077] The method for preparing manganese phosphate provided in this embodiment comprises the following steps:
[0078] Step S1: Mn(NO3)2·4H2O is dissolved in 275 mL of deionized water to prepare Mn 2+ The solution was 60 g / L and stirred in a magnetic heating stirrer at 60 °C;
[0079] Step S2: Press n(Mn 2+ ):n(HClO) molar ratio is 1:0.8. Weigh HClO, add it and NaOH to Mn(NO3)2 solution at the same time and adjust the pH to 8.5. After reacting for 3 hours, filter and wash to obtain MnO(OH) filter cake;
[0080] Step S3: Take an appropriate amount of MnO(OH) filter cake and prepare it into a slurry with a solid content of 15%, place it in a 60°C magnetic heating stirrer for stirring, add H3PO4 to adjust the solution pH to 2.0, react for 3 hours, filter, wash and dry to obtain MnPO4·H2O powder.
[0081] Example 4
[0082] The method for preparing lithium manganese phosphate provided in this embodiment comprises the following steps:
[0083] Step S4: 11.08 g Li2CO3, 50.38 g MnPO4·H2O and 0.60 g sucrose were weighed, keeping the Li / Mn molar ratio at 1 and the C / Mn molar ratio at 0.07, and put them into a 250 mL ball mill together with 110 mL deionized water;
[0084] Step S5: adding zirconium balls of equal mass for ball milling at a rotation speed of 300 r / min for 6 h, and spray drying after completion;
[0085] Step S6: calcine the collected powder at 750°C for 9h under N2 protection and cool naturally to room temperature.
[0086] Comparative Example 1
[0087] The method for preparing manganese phosphate provided in this comparative example is different from that in Example 1 in that step 2, n(Mn 2+ ):n(H2O2) molar ratio is 1:0.5.
[0088] Comparative Example 2
[0089] The method for preparing manganese phosphate provided in this comparative example is different from that in Example 1 in that in step 2, the pH value is adjusted to 6.5.
[0090] Comparative Example 3
[0091] The method for preparing manganese phosphate provided in this comparative example is different from that in Example 1 in that in step 3, the pH value is adjusted to 2.5.
[0092] Experimental example
[0093] The manganese phosphate prepared in Example 1 to Example 3 and Comparative Example 1 to Comparative Example 3 was prepared into lithium manganese phosphate by the preparation method of lithium manganese phosphate provided in Example 4. Then the prepared lithium manganese phosphate was made into lithium ion batteries respectively, and the specific method was as follows: LiMnPO4, Super-P, and PVDF were uniformly dispersed in NMP at a mass ratio of 9:0.5:0.5 to obtain electrode slurry, which was coated on aluminum foil, and then sliced after vacuum drying at 100°C for 12 hours to obtain a positive electrode sheet. With argon as the protective gas, the positive electrode sheet, the metal lithium sheet, the Celgard2325 diaphragm and the 1M LiPF6 ethylene carbonate / diethyl carbonate electrolyte were assembled into a CR2032 button battery in a glove box. The performance of the lithium ion battery was tested by the following methods: constant current and constant voltage charging, cut-off voltage 4.5V, cut-off current 20mA; constant current discharge, cut-off voltage 2.5V.
[0094] Figure 2 This is the XRD spectrum of LiMnPO4 prepared by the method provided in Example 1 and Example 4. From the results, it can be seen that the diffraction peaks of the product correspond one to one with the standard diffraction peaks (PDF#77-0178) of orthorhombic phase LiMnPO4, there is no impure phase peak, the peak intensity is high and the peak shape is sharp, indicating that pure phase LiMnPO4 with good crystallinity is prepared by the above method.
[0095] Table 1 Initial charge and discharge performance of LiMnPO4 prepared from different embodiments and comparative examples
[0096]
[0097]
[0098] Table 1 shows the initial charge and discharge performance of LiMnPO4 prepared by the method provided in Example 4 according to Example 1 to Example 3 and Comparative Example 1 to Comparative Example 3. It can be seen from the results that the discharge specific capacity and initial efficiency of Example 1 to Example 3 at a rate of 0.1C are both over 132.8 mAh·g -1 and 90.0%, with a maximum of 133.2 mAh g -1 and 90.6%, while the discharge specific capacity and first-efficiency maximum values of Comparative Examples 1 to 3 were 128.4 mAh·g -1 and 88.0%, which are lower than those in Example 1 to Example 3, which indicates that the excellent charge and discharge performance of LiMnPO4 can be maximized by reasonably controlling the experimental parameters based on the above-mentioned method for preparing LiMnPO4.
[0099] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A method for preparing manganese phosphate, characterized in that: The following steps are involved: (a) subjecting a mixed solution containing a manganese source, an oxidant and an alkali to a first reaction to obtain MnO(OH); (b) The mixed solution containing MnO(OH) and H3PO4 is subjected to a second reaction to obtain MnPO4·H2O.
2. The method for preparing manganese phosphate according to claim 1, characterized in that: The Mn in the manganese source 2+ The molar ratio of the oxidant to the oxidant is 1:0.7-0.
8.
3. The method for preparing manganese phosphate according to claim 1, characterized in that: The pH of the first reaction is 7.0 to 9.5; And / or, the first reaction time is 2 to 3 hours.
4. The method for preparing manganese phosphate according to claim 1, characterized in that: The pH of the second reaction is 1.6 to 2.0; And / or, the second reaction time is 2 to 3 hours.
5. The method for preparing manganese phosphate according to claim 1, characterized in that: The manganese source includes: divalent manganese salt.
6. The method for preparing manganese phosphate according to claim 5, characterized in that: The divalent manganese salt includes at least one of MnSO4, MnCl2, Mn(NO3)2 or Mn(CH3COO)2.
7. The method for preparing manganese phosphate according to claim 1, characterized in that: The oxidant includes at least one of H2O2, NaClO or HClO.
8. The method for preparing manganese phosphate according to claim 1, characterized in that: The base includes at least one of NaOH, KOH or ammonia water.
9. A method for preparing lithium manganese phosphate, characterized in that: The MnPO4·H2O prepared by the method for preparing manganese phosphate according to any one of claims 1 to 8, a lithium source and a carbon source are ball-milled, spray-dried and calcined to obtain LiMnPO4.
10. A secondary battery, characterized in that: The lithium manganese phosphate prepared by the preparation method of lithium manganese phosphate described in claim 9 is used as the positive electrode material.
Citation Information
Patent Citations
Method for preparing manganese lithium phosphate / carbon composite material by manganese phosphate
CN101673819A
Ferric manganese phosphate and preparation method thereof, lithium ferric manganese phosphate, lithium ion battery and electric equipment