Preparation method of power type ferric sodium pyrophosphate positive electrode material
Through the preparation method of power type sodium iron pyrophosphate positive electrode material, the problem of lithium-ion battery cost and lithium storage limit is solved, and sodium-ion battery materials suitable for electric two-wheelers are provided, with high capacity, good rate performance and low Production cost, suitable as the power battery material for electric two-wheelers.
Patent Information
- Application Number
- CN202411185971.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing lithium-ion batteries have limitations in cost and lithium storage, and electric two-wheelers have high requirements for battery safety and cost. Sodium ion batteries are suitable as electric two-wheelers because of their low raw materials and good safety at high temperatures. The power source of the wheelbarrow, but the research on its sodium storage material has not yet been fully studied.
The preparation method of the power-type sodium ferrous pyrophosphate positive electrode material is prepared by ball milling and spray drying technology, combined with pre-firing and secondary calcining in an inert gas environment, and ferrous oxalate combined with composite iron source, to prepare excellent kinetic properties. Sodium ferric pyrophosphate positive electrode material.
It achieves high capacity, good rate performance and cycle stability, while reducing production costs and improving low temperature performance. It is suitable as a power battery material for electric two-wheelers.
Smart Images

Figure CN119079963A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a method for preparing a power-type sodium iron phosphate pyrophosphate positive electrode material. Background Art
[0002] Energy crisis and environmental change have led to the sustainable development of energy utilization and storage being highly valued by countries around the world. Although lithium-ion batteries have been widely used in small portable electronics, electric vehicles (EVs) or plug-in hybrid electric vehicles (PHEVs), their high cost and limited lithium storage capacity restrict their further development. Sodium-ion batteries are considered to be an ideal large-scale power storage application technology due to their rich sodium resources and environmental friendliness. Therefore, sodium-ion batteries have become a hot research issue in recent years, and various sodium storage materials have been widely studied.
[0003] The development of the new energy industry has attracted attention to the electric two-wheeler market. However, unlike electric cars, which have complete safety devices, electric two-wheelers are more likely to be exposed outdoors for a long time when working, which places higher requirements on battery safety and cost. Compared with lithium-ion batteries, sodium-ion batteries not only have lower raw material prices, but also have better safety because the gas produced by sodium ions at high temperatures is non-flammable. Therefore, sodium-ion batteries are expected to become the next generation of power sources for electric two-wheelers. Summary of the invention
[0004] In view of the above problems existing in the prior art, the present invention provides a method for preparing a power-type sodium iron pyrophosphate positive electrode material, which is used to overcome the above defects in the prior art.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing a power-type sodium iron phosphate pyrophosphate positive electrode material comprises the following steps:
[0007] The first step is to add a sodium source, an iron source and a phosphorus source into a ball mill at a ratio of 4: (2.9-3): 4, prepare zirconium balls at a ball-to-material ratio of 1:20, add a ball milling medium solvent at a ratio of 2-4 kg / L, and then add a first carbon source at a weight of 2-4% of the weight of the sodium source and iron source, ball milling to make the slurry particle size reach 2-4 μm, and spray drying to obtain a first spray material;
[0008] In the second step, the first spray material obtained in the first step is pre-burned in an inert gas environment using a roller furnace, and then the pre-burned material is air flow crushed and vibrated through a sieve of 80 to 120 meshes to obtain a NFPP pre-burned material;
[0009] The third step is to add the NFPP pre-sintered material prepared in the second step into a ball mill, and then add a second carbon source according to 1.5-3% of the mass of the NFPP pre-sintered material and an additive according to 0.5-1.5% of the mass of the NFPP pre-sintered material, add zirconium balls prepared at a ball-to-material ratio of 1:20, add an appropriate amount of ball milling medium solvent at a ratio of 5-7kg / L, ball mill the slurry to a particle size of 1-2μm, and spray dry to obtain a second spray material;
[0010] In the fourth step, the second spray material obtained in the third step is calcined in an inert gas atmosphere using a roller furnace to obtain a power-type sodium iron phosphate pyrophosphate positive electrode material.
[0011] In one embodiment, the sodium source is one or more of sodium dihydrogen phosphate, sodium carbonate, sodium bicarbonate, sodium acetate, and sodium pyrophosphate;
[0012] The iron source is one or more of ferrous oxalate, ferrous phosphate, ferrous acetate, ferrous sulfate, and ferrous nitrate.
[0013] The phosphorus source is one or more of ammonium phosphate, diammonium phosphate, and ammonium hydrogen phosphate.
[0014] In one embodiment, the first carbon source is one or more of glucose, sucrose, citric acid, ascorbic acid, polyethylene glycol 400-800;
[0015] The second carbon source is one or more of glucose, sucrose, citric acid, ascorbic acid, and polyethylene glycol 800-4000.
[0016] In one embodiment, the additive is one of ethylene glycol, stearic acid, oleic acid, sodium fatty alcohol sulfate, and carboxy betaine.
[0017] In one of the embodiments, the heating rate of the pre-firing operation is 10-20°C / min, the pre-firing temperature is 450-500°C, the time in the high temperature zone is 3-6h, and the cooling rate in the cooling zone is 5-10°C / min.
[0018] In one embodiment, the calcination operation is to increase the temperature to 400-450°C at a rate of 5-10°C / min and keep it at that temperature for 2 hours, and then increase the temperature to 500-580°C and keep it at that temperature for 10-12 hours.
[0019] In one embodiment, the spray drying operation in the first step has a spray speed of 10,000 to 12,000 rpm and a temperature of 80 to 90° C.
[0020] The spraying speed of the spray drying operation in the third step is between 9000 and 11000 rpm and the temperature is between 85 and 100°C.
[0021] In one embodiment, the mass of the first carbon source in the first step is 2%, the mass of the second carbon source in the third step is 1.5%, and the mass of the additive is 0.5%.
[0022] In one embodiment, the ball milling medium is one of methanol, ethanol or water.
[0023] Compared with the prior art, the present invention provides a method for preparing a power-type sodium iron phosphate pyrophosphate positive electrode material. By using ferrous oxalate in combination with a composite iron source and a sodium source, spray drying and secondary calcination, the sodium iron phosphate pyrophosphate positive electrode material is prepared by a solid phase ball milling spray drying method. A sodium iron phosphate pyrophosphate power battery with excellent kinetic performance can be quickly prepared. The battery has high capacity and good rate performance, as well as good cycle stability, low production cost, and excellent cycle performance and low temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a comparison chart of the particle size peak types of Example 1 and the comparative example provided by the present invention. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments:
[0026] Example 1
[0027] (1) adding sodium carbonate, ferrous nitrate and ammonium phosphate into a ball mill at a ratio of Na:Fe:P=4:2.95:4, preparing zirconium balls at a ball-to-material ratio of 1:20, adding anhydrous ethanol at a ratio of 3 kg / L, adding glucose at a weight of 2% of the weight of the sodium source and the iron source, ball milling for a certain period of time to make the slurry particle size reach 2 to 4 μm, spray drying to obtain a first spray material, wherein the spraying speed of the spray drying operation is between 10,000 and 12,000 rpm and the temperature is between 80 and 90° C.;
[0028] (2) Pre-calcining the first spray material obtained in (1) in an argon atmosphere using a roller furnace, with a heating rate of 10°C / min to a temperature of 450°C, keeping the temperature in the high temperature zone for 3 hours and then entering the cooling zone, controlling the cooling rate in the cooling zone to make the material cooling rate in the range of 5 to 10°C / min, and then air-grinding the pre-calcined material, and vibrating and sieving it through a 100-mesh sieve to obtain a NFPP pre-calcined material;
[0029] (3) The NFPP pre-sintered material prepared in (2) is added into a ball mill, and then polyethylene glycol 1000 is added at 1.5% of the mass of the NFPP pre-sintered material and stearic acid is added at 0.5% of the mass of the NFPP pre-sintered material, zirconium balls are prepared at a ball-to-material ratio of 1:20, anhydrous ethanol is added at a ratio of 5 kg / L, the slurry is ball-milled to a particle size of 1 to 2 μm, and a second spray material is obtained by spray drying. The spray speed of the spray drying operation is between 9000 and 11000 rpm and the temperature is between 85 and 100° C., and then the second spray material is calcined in an argon atmosphere, and the temperature is increased to 450° C. at a rate of 10° C. / min and kept for 2 h, and then the temperature is increased to 550° C. and kept for 10 h, thereby obtaining a power-type sodium iron phosphate pyrophosphate positive electrode material.
[0030] Example 2
[0031] (1) adding sodium dihydrogen phosphate, ferrous oxalate and sodium carbonate into a ball mill at a ratio of Na:Fe:P=4:2.95:4, preparing zirconium balls at a ball-to-material ratio of 1:20, adding anhydrous ethanol at a ratio of 3 kg / L, adding glucose at a mass ratio of 2% of the sodium source and iron source, ball milling for a certain period of time to make the slurry particle size reach 2-4 μm, spray drying to obtain a first spray material, the spraying speed of the spray drying operation is between 10,000 and 12,000 rpm, and the temperature is between 80 and 90° C.;
[0032] (2) using a roller furnace to pre-sinter the first spray material obtained in (1) under an argon atmosphere, with a heating rate of 10°C / min to a temperature of 450°C, keeping the temperature in the high temperature zone for 3 hours and then entering the cooling zone, controlling the cooling rate in the cooling zone to make the material cooling rate in the range of 5 to 10°C / min, and then air-grinding the pre-sintered material, and vibrating and sieving it through a 100-mesh sieve to obtain a NFPP pre-sintered material;
[0033] (3) The NFPP pre-sintered material prepared in (2) is added to a ball mill, and then polyethylene glycol 1000 is added at 1.5% of the mass of the NFPP pre-sintered material, and stearic acid is added at 0.5% of the mass of the NFPP pre-sintered material, zirconium balls are prepared at a ball-to-material ratio of 1:20, and anhydrous ethanol is added at a ratio of 5kg / L. The ball-milled slurry is subjected to a particle size of 1 to 2 μm, and spray-dried to obtain a second spray material, the spray speed of the spray drying operation is between 9000 and 11000 rpm, and the temperature is between 85 and 100°C. The second spray material is then calcined in an argon atmosphere, heated to 450°C at a rate of 10°C / min and kept warm for 2 hours, and then heated to 550°C and kept warm for 10 hours, thereby obtaining a power-type sodium iron phosphate pyrophosphate positive electrode material.
[0034] Example 3
[0035] (1) adding sodium carbonate, ferric phosphate, sodium pyrophosphate, and ammonium phosphate into a ball mill at a ratio of Na:Fe:P=4:2.95:4, preparing zirconium balls at a ball-to-material ratio of 1:20, adding anhydrous ethanol at a ratio of 3 kg / L, adding glucose at a weight of 2% of the mass of the sodium source and the iron source, ball milling for a certain period of time to make the slurry particle size reach 2 to 4 μm, and spray drying to obtain a first spray material, wherein the spraying speed of the spray drying operation is between 10,000 and 12,000 rpm and the temperature is between 80 and 90° C.;
[0036] (2) using a roller furnace to pre-sinter the first spray material obtained in (1) under an argon atmosphere, with a heating rate of 10°C / min to a temperature of 450°C, keeping the temperature in the high temperature zone for 3 hours and then entering the cooling zone, controlling the cooling rate in the cooling zone to make the material cooling rate in the range of 5 to 10°C / min, and then air-grinding the pre-sintered material, and vibrating and sieving it through a 100-mesh sieve to obtain a NFPP pre-sintered material;
[0037] (3) The NFPP pre-sintered material prepared in (2) is added to a ball mill, and then polyethylene glycol 1000 is added at 1.5% of the mass of the NFPP pre-sintered material, and stearic acid is added at 0.5% of the mass of the NFPP pre-sintered material, zirconium balls are prepared at a ball-to-material ratio of 1:20, and anhydrous ethanol is added at a ratio of 5kg / L. The ball milled slurry has a particle size of 1-2μm, and spray-dried to obtain a second spray material, the spray speed of the spray drying operation is between 9000 and 11000rpm, and the temperature is between 85 and 100°C, and then the second spray material is calcined in an argon atmosphere, and the temperature is increased to 450°C at a rate of 10°C / min and kept for 2h, and then the temperature is increased to 550°C and kept for 10h, thereby obtaining a power-type sodium iron phosphate pyrophosphate positive electrode material.
[0038] Comparative Example 1:
[0039] (1) adding sodium dihydrogen phosphate, ferrous oxalate and sodium carbonate into a ball mill at a ratio of Na:Fe:P=4:2.95:4, preparing zirconium balls at a ball-to-material ratio of 1:20, adding anhydrous ethanol at a ratio of 3 kg / L, adding glucose at a mass ratio of 2% of the sodium source and iron source, ball milling for a certain period of time to make the slurry particle size reach 2-4 μm, spray drying to obtain a first spray material, the spraying speed of the spray drying operation is between 10,000 and 12,000 rpm, and the temperature is between 80 and 90° C.;
[0040] (2) using a roller furnace to pre-sinter the first spray material obtained in (1) under an argon atmosphere, with a heating rate of 10°C / min to a temperature of 450°C, keeping the temperature in the high temperature zone for 3 hours and then entering the cooling zone, controlling the cooling rate in the cooling zone to make the material cooling rate in the range of 5 to 10°C / min, and then air-grinding the pre-sintered material, and vibrating and sieving it through a 100-mesh sieve to obtain a NFPP pre-sintered material;
[0041] (3) The NFPP pre-sintered material prepared in (2) is added to a ball mill, and zirconium balls are directly prepared according to a ball-to-material ratio of 1:20. Anhydrous ethanol is added at a ratio of 5 kg / L, and the slurry is ball-milled to a particle size of 1 to 2 μm. The second spray material is spray-dried, and the spray speed of the spray drying operation is between 9000 and 11000 rpm and the temperature is between 85 and 100° C. The second spray material is then calcined in an argon atmosphere, and the temperature is increased to 450° C. at a rate of 10° C. / min and kept for 2 h, and then increased to 550° C. and kept for 10 h, thereby obtaining a power-type sodium iron pyrophosphate positive electrode material.
[0042] Button test: The prepared sodium iron phosphate pyrophosphate and SP, PVDF were mixed and ground evenly in a ratio of 9:0.5:0.5, a certain amount of NMP was added, stirred and slurried, and then coated and dried. GF diaphragm and NaClO4 electrolyte were used to prepare 2032 button batteries. The charge and discharge capacity of 0.1-0.5-1C was tested in the range of 2-4V. The results are shown in the following table:
[0043]
[0044] From the comparison of electrical properties in the above table, it can be seen that the sodium iron phosphate pyrophosphate positive electrode material with a composite carbon coating structure prepared by the preparation method provided by the present invention through two-step calcination has a higher rate performance, and the selection of the main material sodium / iron / phosphorus source will have a certain impact on the performance. Comparative Example 1 proves that when ball milling NFPP pre-sintered material, if no additional carbon source and additives are added, the electrical performance will be greatly reduced. Figure 1 It can be seen from the particle size peak diagram that the particle size of Comparative Example 1, which is also ball milled for 2 hours but without adding additives, is much larger than that of Example 1.
[0045] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0046] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a power-type sodium iron phosphate pyrophosphate positive electrode material, characterized in that: The following steps are involved: The first step is to add a sodium source, an iron source and a phosphorus source into a ball mill at a ratio of 4: (2.9-3): 4, prepare zirconium balls at a ball-to-material ratio of 1:20, add a ball milling medium solvent at a ratio of 2-4 kg / L, and then add a first carbon source at a weight of 2-4% of the weight of the sodium source and iron source, ball milling to make the slurry particle size reach 2-4 μm, and spray drying to obtain a first spray material; In the second step, the first spray material obtained in the first step is pre-burned in an inert gas environment using a roller furnace, and then the pre-burned material is air flow crushed and vibrated through a sieve of 80 to 120 meshes to obtain a NFPP pre-burned material; The third step is to add the NFPP pre-sintered material prepared in the second step into a ball mill, and then add a second carbon source according to 1.5-3% of the mass of the NFPP pre-sintered material and an additive according to 0.5-1.5% of the mass of the NFPP pre-sintered material, add zirconium balls prepared at a ball-to-material ratio of 1:20, add an appropriate amount of ball milling medium solvent at a ratio of 5-7kg / L, ball mill the slurry to a particle size of 1-2μm, and spray dry to obtain a second spray material; In the fourth step, the second spray material obtained in the third step is calcined in an inert gas atmosphere using a roller furnace to obtain a power-type sodium iron phosphate pyrophosphate positive electrode material.
2. A method for preparing a power-type sodium iron pyrophosphate positive electrode material as claimed in claim 1, characterized in that: The sodium source is one or more of sodium dihydrogen phosphate, sodium carbonate, sodium bicarbonate, sodium acetate, and sodium pyrophosphate; The iron source is one or more of ferrous oxalate, ferrous phosphate, ferrous acetate, ferrous sulfate, and ferrous nitrate. The phosphorus source is one or more of ammonium phosphate, diammonium phosphate, and ammonium hydrogen phosphate.
3. The method for preparing a power-type sodium iron pyrophosphate positive electrode material according to claim 1, characterized in that: The first carbon source is one or more of glucose, sucrose, citric acid, ascorbic acid, and polyethylene glycol 400-800; The second carbon source is one or more of glucose, sucrose, citric acid, ascorbic acid, and polyethylene glycol 800-4000.
4. The method for preparing a power-type sodium iron pyrophosphate positive electrode material according to claim 1, characterized in that: The additive is one of ethylene glycol, stearic acid, oleic acid, sodium fatty alcohol sulfate, and carboxy betaine.
5. A method for preparing a power-type sodium iron phosphate pyrophosphate positive electrode material as claimed in claim 1, characterized in that: The heating rate of the pre-burning operation is 10-20°C / min, the pre-burning temperature is 450-500°C, the time in the high temperature zone is 3-6h, and the cooling rate in the cooling zone is 5-10°C / min.
6. A method for preparing a power-type sodium iron pyrophosphate positive electrode material according to claim 1, characterized in that: The calcination operation is to heat up to 400-450° C. at a rate of 5-10° C. / min and keep the temperature for 2 hours, and then heat up to 500-580° C. and keep the temperature for 10-12 hours.
7. The method for preparing a power-type sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The spray drying process in the first step has a spray speed of 10,000 to 12,000 rpm and a temperature of 80 to 90° C. The spraying speed of the spray drying operation in the third step is between 9000 and 11000 rpm and the temperature is between 85 and 100°C.
8. The method for preparing a power-type sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The mass of the first carbon source in the first step is 2%, the mass of the second carbon source in the third step is 1.5% and the mass of the additive is 0.5%.
9. The method for preparing a power-type sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The ball milling medium is one of methanol, ethanol or water.
Citation Information
Patent Citations
Porous ferric sodium pyrophosphate / carbon composite material as well as preparation method and application thereof
CN116799131A
Low-cost preparation method of polyanion positive electrode material
CN117776137A
Preparation method of high-specific-energy ferric sodium pyrophosphate positive electrode material
CN118156463A
Carbon-coated ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof
CN118213528A
Iron-based sodium ion full battery and preparation method therefor
WO2024011862A1