Preparation method of superfine low-sodium low-silicon aluminum oxide powder and application of superfine low-sodium low-silicon aluminum oxide powder in battery diaphragm
By extracting, separating and grinding the industrial alumina, the problem of high sodium and silicon impurities in the lithium battery separator is solved, and low-cost, high-purity ultra-fine low-sodium low-silicon alumina powder is prepared, suitable for battery separator coatings , improves the safety and performance of lithium batteries.
Patent Information
- Application Number
- CN202411292238.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
AI Technical Summary
The alumina products in existing lithium battery separators have high sodium and silicon impurities, which affect battery performance and safety. The high-purity alumina preparation cost is high, which limits industrial mass production.
By extracting and separating the industrial alumina after ball milling, extracting and processing using a mixed solvent of ethanol and n-hexane, sodium and silicon impurities in the alumina are removed in a directionally to obtain high-purity ultrafine low-sodium low-silicon alumina powder, and Products suitable for battery separator coatings are obtained by grinding.
It realizes the preparation of low-cost, high-purity ultra-fine low-sodium low-silicon aluminum oxide powder, reduces the preparation cost of alumina-coated separators, is suitable for industrial production, and improves the safety and performance of lithium batteries.
Smart Images

Figure CN119080039A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional materials, and in particular to a method for preparing ultrafine low-sodium and low-silicon alumina powder and application thereof in battery separators. Background Art
[0002] With the rapid development of new energy vehicles and energy storage, the demand for lithium-ion batteries continues to grow, and the performance requirements for lithium batteries continue to increase. As a vital component of modern electric vehicles and renewable energy storage, the safety and performance of lithium batteries are crucial to the development of the entire industry chain and the safety of users. Separators are a key technology for improving the safety of lithium batteries. Currently, commonly used lithium battery separators are mainly made of polyolefin materials such as polyethylene (PE) and polypropylene (PP). As the capacity of lithium battery rechargeable cells continues to increase, the accumulated energy causes the battery temperature to rise, causing the separator to melt and short circuit. Because alumina has insulating, heat-insulating, and high-temperature resistant properties, it is often coated on the separator surface to improve its heat resistance and mechanical strength. Alumina-coated ceramic separators offer advantages such as high temperature resistance, high safety, high rate capability, good wettability, self-shutoff characteristics, low self-discharge rate, and long cycle life. However, alumina products currently on the market have high levels of impurities such as sodium and silicon, which can affect the performance and safety of lithium batteries. For example, the presence of sodium impurities can affect the performance of lithium batteries in several ways, as follows:
[0003] 1. Impact on electrode material structure: Sodium present in the separator coating may embed into the cathode material lattice during the battery's charge and discharge process. For example, in ternary cathode materials, if sodium ions occupy lithium ion sites, they will cause lattice defects in the cathode material, change the material's crystal structure, and hinder the insertion and extraction of lithium ions, resulting in a decrease in the battery's charge and discharge capacity. This effect is often irreversible.
[0004] 2. Interference with internal battery reactions: During the battery charge and discharge process, sodium may participate in some side reactions. For example, sodium may react with the electrolyte to form compounds that are not conducive to the normal operation of the battery. These compounds may clog the electrode pores, hinder the transmission channels of lithium ions, increase the internal resistance of the battery, and affect the battery's rate performance (i.e., the battery's performance when charging and discharging at high currents).
[0005] 3. Reduced battery energy density: Sodium has a relatively large atomic mass and ionic radius. Compared to lithium ions, sodium ions can store relatively less charge in the same mass or volume of electrode material. This means that the presence of sodium impurities will reduce the energy that can be stored per unit mass or volume of the battery, reducing the battery's energy density and affecting its battery life.
[0006] The impact of silicon impurities on lithium battery performance is mainly reflected in the following aspects:
[0007] 1. Causes electrode volume changes: Silicon undergoes alloying and dealloying reactions with lithium ions during the charge and discharge process, accompanied by a huge volume expansion (up to 300%-400%). When silicon exists as an impurity, its uneven distribution in the electrode or high local content will cause uneven volume changes in the electrode during the cycle. This uneven volume expansion will cause stress in the electrode structure, causing the electrode material to crack and pulverize, and fall off the electrode sheet, thereby reducing the active material that can participate in the electrochemical reaction, causing the battery capacity to decline sharply and shortening the cycle life.
[0008] 2. Destruction of the solid electrolyte interface (SEI) film: During battery cycling, the volume change of silicon continuously creates new surfaces, causing the SEI film to be repeatedly destroyed and rebuilt. The formation and stability of the SEI film are crucial to battery performance. Its repeated changes will continuously consume lithium and electrolyte from the positive electrode, ultimately leading to an increase in the battery's internal resistance and a rapid decrease in capacity.
[0009] 3. Impact on battery rate performance: Silicon material has relatively poor conductivity. When present as an impurity, it will reduce the overall conductivity of the electrode to a certain extent. The transmission of electrons and the diffusion of lithium ions in the silicon impurity area will be hindered, making it difficult for the battery to withstand large charge and discharge currents, showing poor rate performance, that is, the battery performance decreases when charging and discharging at high currents.
[0010] To obtain high-purity alumina, two methods are currently used: using high-purity alumina as a seed crystal, hydrolyzing aluminum alcoholate, and then sintering it; or adding high-purity alumina to the resulting aluminum hydroxide sol for a hydrothermal reaction, followed by high-temperature sintering of the hydrothermal reaction product to obtain high-purity alumina. These methods are characterized by high cost and complex processes, making them unsuitable for industrial mass production, limiting their practical application in lithium battery separators.
[0011] Based on this, there is an urgent need for a method that can produce ultrafine high-purity alumina powder at low cost and suitable for batch production to reduce the preparation cost of alumina-coated diaphragms. Summary of the Invention
[0012] The present invention provides a method for preparing ultrafine low-sodium, low-silicon alumina powder and its application in battery separators, so as to solve the problems of high sodium and silicon contents in the current alumina used for lithium battery separators and high preparation cost of high-purity alumina. The present invention extracts and separates the industrial alumina after ball milling to carry out targeted impurity removal of silicon and sodium impurities in the alumina without almost affecting the main body of the alumina, so that the alumina obtained after the above treatment has low content of silicon and sodium impurities and small and uniform particle size, which is suitable for preparing battery separator coatings.
[0013] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0014] A first aspect of the present invention provides a method for preparing ultrafine low-sodium and low-silicon alumina powder, comprising the following steps:
[0015] (1) ball milling industrial alumina to obtain alumina powder;
[0016] (2) dispersing the alumina powder prepared in step (1) in water to obtain an alumina dispersion; mixing and stirring the alumina dispersion with an extractant to obtain an alumina mixed solution; centrifuging and separating the alumina mixed solution to obtain an alumina slurry; the extractant is a mixed solvent of ethanol and n-hexane;
[0017] (3) Grinding the alumina slurry and drying it to obtain the ultrafine low-sodium and low-silicon alumina powder.
[0018] Furthermore, in step (1), the industrial alumina is a block or granular solid.
[0019] Furthermore, in step (1), the D50 of the industrial alumina is 30-40 μm.
[0020] Furthermore, in step (1), the purity of the industrial alumina is ≦99.7%, the silicon content is ≧0.05%, and the sodium content is ≧0.17%.
[0021] Furthermore, in step (1), the industrial alumina is dried and then ball-milled; the drying temperature is 100-110° C. and the time is 1-2 hours.
[0022] Furthermore, in step (1), in the ball milling step: the ball milling medium is alumina balls, the ball-to-material ratio is preferably 5-7:1, the ball milling speed is preferably 400-500 rpm, and the ball milling time is preferably 3-6 h; preferably, the ball milling medium is obtained by mixing alumina balls with diameters of 10 mm, 8 mm, 5 mm, and 3 mm in a mass ratio of 1:2:3:4; in some preferred embodiments, the ball milling is first performed at a speed of 500 rpm for 2-3 h, and then at a speed of 400 rpm for 1-3 h.
[0023] Furthermore, in step (1), the ball-milled aluminum oxide powder is sieved to ensure uniform particle size.
[0024] Furthermore, in step (1), the particle size of the alumina powder is preferably 1-2 μm. The particle size of the industrial alumina is reduced by ball milling to increase the contact area between the alumina powder and the extractant during the extraction process. However, the particle size of the alumina powder cannot be too low. Alumina with too fine particles is prone to agglomeration during subsequent treatment, thereby affecting the impurity removal effect. Preferably, the particle size of the industrial alumina is controlled to be in the range of 1-2 μm by ball milling.
[0025] Furthermore, in step (2), the solid content of the alumina dispersion is preferably 20%-40%, for example 30%; and the volume ratio of the alumina dispersion to the extractant is preferably (1-3):1.
[0026] Furthermore, in step (2), the volume ratio of ethanol to n-hexane in the extractant is preferably 1:(3-5); the extractant prepared by ethanol and n-hexane in a certain volume ratio is used to extract industrial alumina, so that silicon-containing and sodium-containing impurities in the industrial alumina enter the organic phase, and the impurities and alumina can be separated by simple phase separation; however, the volume ratio of ethanol to n-hexane in the extractant needs to be controlled within a certain range, for example, 1:3-5. If the ethanol ratio is too low, the impurity removal effect is poor, but if the ethanol ratio is too high, the polarity of the extraction system will be too large, affecting the extraction effect of the target impurities and subsequent stratification.
[0027] Furthermore, in step (2), the mixing and stirring temperature is 20-50° C., and the mixing and stirring time is 30-60 min.
[0028] Furthermore, in step (2), the centrifugal speed is 100-200 rpm and the time is 15 min-1 h.
[0029] Furthermore, in step (2), the step of separating the liquids is specifically as follows: the alumina mixed liquid after centrifugation is allowed to stand for a period of time, and after standing for separation, an alumina slurry in the lower layer is obtained.
[0030] Furthermore, in step (3), in the grinding treatment step: the grinding medium is alumina beads, the ball-to-material ratio is 5-10:1, the grinding speed is 1500-3000 rpm, and the grinding time is 4-6h; more preferably, the diameter of the alumina beads is 0.3-0.6mm.
[0031] Furthermore, in step (3), the drying temperature is 100-120° C. and the drying time is 2-4 hours, for example, drying at 110° C. for 3 hours.
[0032] The second aspect of the present invention provides an ultrafine low-sodium and low-silicon alumina powder prepared by the preparation method described in the first aspect.
[0033] Furthermore, the average particle size of the ultrafine low sodium and low silicon alumina powder is 200-500 nm; the alumina content of the ultrafine low sodium and low silicon alumina powder is ≥99.9%, the sodium content is ≤0.05%, and the silicon content is <0.05%.
[0034] The third aspect of the present invention provides a battery separator comprising a base film and a coating provided on at least one side of the base film along the thickness direction; the coating comprises the ultrafine low-sodium and low-silicon alumina powder described in the second aspect.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. Unlike the existing technology that uses high-cost aluminum alcohol salts or aluminum hydroxide as raw materials and uses high-purity alumina as seed crystals to obtain high-purity alumina through hydrolysis / hydrothermal reaction and sintering. The present invention uses low-cost industrial alumina as raw material, appropriately increases the specific surface area of the alumina particles through ball milling, and avoids agglomeration caused by excessive particle refinement. The ball-milled alumina powder is then extracted with an extractant prepared from ethanol and n-hexane in a certain volume ratio. The extractant reacts with the alumina but can selectively remove silicon and sodium impurities in the alumina. After further grinding, a high-purity, low-sodium, low-silicon ultrafine alumina powder can be obtained.
[0037] 2. The method provided by the present invention for preparing ultrafine low-sodium, low-silicon alumina powder is simple to operate and has low production costs. It requires only ball milling, extraction, and grinding to produce high-purity ultrafine silicon alumina powder, making it suitable for industrial production. The ultrafine alumina powder prepared by this method has an alumina content of ≥99.9%, a sodium content of ≤0.05%, and a silicon content of ≤0.02%, making it suitable for preparing battery separator coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is the particle size distribution diagram of industrial alumina;
[0039] Figure 2 is the particle size distribution diagram of the alumina powder after ball milling in Example 1;
[0040] Figure 3 This is the particle size distribution diagram of the ultrafine low sodium and low silicon alumina powder prepared in Example 1;
[0041] Figure 4 This is the particle size distribution diagram of the ultrafine low sodium and low silicon alumina powder prepared in Example 2;
[0042] Figure 5 This is the particle size distribution diagram of the ultrafine low sodium and low silicon alumina powder prepared in Example 3;
[0043] Figure 6This is the particle size distribution diagram of the ultrafine alumina powder prepared in Comparative Example 1;
[0044] Figure 7 This is the particle size distribution diagram of the ultrafine alumina powder prepared in Comparative Example 2;
[0045] Figure 8 This is the particle size distribution diagram of the ultrafine alumina powder prepared in Comparative Example 3. DETAILED DESCRIPTION
[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention pertains. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the relevant listed items. The term "includes" or "comprising" described in the present invention means that in addition to the components described, it may also include or contain other components. The term "includes" or "comprising" described in the present invention may also be replaced by the closed form "for" or "consisting of..."
[0047] The present invention will be further described below with reference to specific embodiments and accompanying drawings so that those skilled in the art can better understand and implement the present invention. However, the embodiments are not intended to limit the present invention.
[0048] The industrial alumina raw materials used in the following examples and comparative examples were purchased from Shandong Zibo Noda Chemical Co., Ltd., model ND-01.
[0049] Example 1
[0050] This embodiment relates to the preparation of an ultrafine low-sodium, low-silicon alumina powder, as follows:
[0051] (1) A certain amount of industrial alumina (D50 of 31.83 μm) was spread in an oven and dried at 100-110°C for 1-2 hours to obtain a dried alumina sample. The dried alumina was ball-milled with a ball-to-material ratio of 6:1. The ball-milling medium was alumina balls with diameters of 10 mm, 8 mm, 5 mm, and 3 mm in a mass ratio of 1:2:3:4. The alumina powder was first ball-milled at 500 rpm for 2 hours and then at 400 rpm for 2 hours to obtain alumina powder with a D50 of 12.99 μm.
[0052] (2) According to the volume ratio of ethanol to n-hexane being 1:3, 50 mL of ethanol and 150 mL of n-hexane are added to the container in sequence, and the volume ratio of the extractant to the alumina dispersion is 1:3; the pretreated alumina powder is prepared into 600 mL of alumina dispersion according to a solid content of 30%, and added to the above container, and placed on a constant temperature magnetic stirrer, stirred at 30°C for 60 minutes, and set aside.
[0053] The stirred alumina mixture was added to a centrifuge test tube and placed in a centrifuge at 150 rpm for 30 minutes. After centrifugation, the alumina mixture in the centrifuge test tube was taken out and added to a separatory funnel for separation. After standing and stratification, the lower layer of alumina slurry was flowed out from the lower mouth of the separatory funnel into a beaker to obtain alumina slurry.
[0054] (3) Add the alumina slurry into a horizontal sand mill for grinding, using alumina beads as the grinding medium, with a diameter of 0.3-0.6 mm, a ball-to-material ratio of 5:1, grinding for 6 hours, and a grinding speed of 2000 rpm; the ground ultrafine alumina slurry is dried at 110° C. for 3 hours to obtain ultrafine low-sodium, low-silicon alumina.
[0055] X-ray fluorescence spectrometry (XRF) was used to test the content of each element, and the test results were as follows: the content of aluminum oxide in the product was 99.95%, the content of sodium was 0.03%, the content of silicon was 0.01%, and the rest were other impurities.
[0056] The particle size of the powder was tested using a laser particle size analyzer, and the average particle size D50 was 0.252 μm.
[0057] Example 2
[0058] This embodiment relates to the preparation of an ultrafine low-sodium, low-silicon alumina powder. The difference from Example 1 is that the volume ratio of ethanol to n-hexane in the extractant is as follows:
[0059] (1) A certain amount of industrial alumina (D50 of 31.83 μm) was spread in an oven and dried at 100-110°C for 1-2 hours to obtain a dried alumina sample. The dried alumina was ball-milled with a ball-to-material ratio of 6:1. The ball-milling medium was alumina balls with diameters of 10 mm, 8 mm, 5 mm, and 3 mm in a mass ratio of 1:2:3:4. The alumina powder was first ball-milled at 500 rpm for 2 hours and then at 400 rpm for 2 hours to obtain alumina powder with a D50 of 12.99 μm.
[0060] (2) According to the volume ratio of ethanol to n-hexane being 1:4, 50 mL of ethanol and 200 mL of n-hexane are added to the container in sequence, and the volume ratio of the extractant to the alumina dispersion is 1:3; the pretreated alumina powder is prepared into 750 mL of alumina dispersion according to a solid content of 30%, and added to the above container, and placed on a constant temperature magnetic stirrer, stirred at 30°C for 60 minutes, and set aside.
[0061] The stirred alumina mixture was added to a centrifuge test tube and placed in a centrifuge at 150 rpm for 30 minutes. After centrifugation, the alumina mixture in the centrifuge test tube was taken out and added to a separatory funnel for separation. After standing and stratification, the lower layer of alumina slurry was flowed out from the lower mouth of the separatory funnel into a beaker to obtain alumina slurry.
[0062] (3) Add the alumina slurry into a horizontal sand mill for grinding, using alumina beads as the grinding medium, with a diameter of 0.3-0.6 mm, a ball-to-material ratio of 5:1, grinding for 6 hours, and a grinding speed of 2000 rpm; the ground ultrafine alumina slurry is dried at 110° C. for 3 hours to obtain ultrafine low-sodium, low-silicon alumina.
[0063] X-ray fluorescence spectrometry (XRF) was used to test the content of each element, and the test results were as follows: the content of aluminum oxide in the product was 99.92%, the content of sodium was 0.04%, the content of silicon was 0.03%, and the rest were other impurities.
[0064] The particle size of the powder was tested using a laser particle size analyzer, and the average particle size D50 was 0.394 μm.
[0065] Example 3
[0066] This embodiment relates to the preparation of an ultrafine low-sodium, low-silicon alumina powder. The difference from Example 2 is that the grinding time is as follows:
[0067] (1) A certain amount of industrial alumina (D50 of 31.83 μm) was spread in an oven and dried at 100-110°C for 1-2 hours to obtain a dried alumina sample. The dried alumina was ball-milled with a ball-to-material ratio of 6:1. The ball-milling medium was alumina balls with diameters of 10 mm, 8 mm, 5 mm, and 3 mm in a mass ratio of 1:2:3:4. The alumina powder was first ball-milled at 500 rpm for 2 hours and then at 400 rpm for 2 hours to obtain alumina powder with a D50 of 12.99 μm.
[0068] (2) According to the volume ratio of ethanol to n-hexane being 1:4, 50 mL of ethanol and 200 mL of n-hexane are added to the container in sequence, and the volume ratio of the extractant to the alumina dispersion is 1:3; the pretreated alumina powder is prepared into 750 mL of alumina dispersion according to a solid content of 30%, and added to the above container, and placed on a constant temperature magnetic stirrer, stirred at 30°C for 60 minutes, and set aside.
[0069] The stirred alumina mixture was added to a centrifuge test tube and placed in a centrifuge at 150 rpm for 30 minutes. After centrifugation, the alumina mixture in the centrifuge test tube was taken out and added to a separatory funnel for separation. After standing and stratification, the lower layer of alumina slurry was flowed out from the lower mouth of the separatory funnel into a beaker to obtain alumina slurry.
[0070] (3) Add the alumina slurry into a horizontal sand mill for grinding, using alumina beads as the grinding medium, with a diameter of 0.3-0.6 mm, a ball-to-material ratio of 5:1, grinding for 4 hours, and a grinding speed of 2000 rpm; the ground ultrafine alumina slurry is dried at 110° C. for 3 hours to obtain ultrafine low-sodium, low-silicon alumina.
[0071] X-ray fluorescence spectrometry (XRF) was used to test the content of each element, and the test results were as follows: the content of aluminum oxide in the product was 99.9%, the content of sodium was 0.05%, the content of silicon was 0.04%, and the rest were other impurities.
[0072] The particle size of the powder was measured using a laser particle size analyzer, and the average particle size D50 was 0.515 μm.
[0073] Comparative Example 1
[0074] This comparative example relates to the preparation of an ultrafine alumina powder, which is specifically as follows:
[0075] A certain amount of industrial alumina (D50: 31.83 μm) was spread flat in an oven and dried at 100-110°C for 1-2 hours to obtain a dried alumina sample. The dried alumina was then ground in a horizontal sand mill using alumina beads with a diameter of 0.3-0.6 mm, a ball-to-bearing ratio of 10:1, and a grinding speed of 2000 rpm for 6 hours to obtain the alumina.
[0076] X-ray fluorescence spectrometry (XRF) was used to test the content of each element, and the test results were as follows: the content of aluminum oxide in the product was 99.6%, the content of sodium was 0.3%, the content of silicon was 0.09%, and the rest were other impurities.
[0077] The particle size of the powder was measured using a laser particle size analyzer, and the average particle size was 2.688 μm.
[0078] Comparative Example 2
[0079] This comparative example relates to the preparation of ultrafine alumina powder, which differs from Example 1 in that the extractant is ethanol, specifically:
[0080] (1) A certain amount of industrial alumina (D50 of 31.83 μm) was spread in an oven and dried at 100-110°C for 1-2 hours to obtain a dried alumina sample. The dried alumina was ball-milled with a ball-to-material ratio of 6:1. The ball-milling medium was alumina balls with diameters of 10 mm, 8 mm, 5 mm, and 3 mm in a mass ratio of 1:2:3:4. The alumina powder was first ball-milled at 500 rpm for 2 hours and then at 400 rpm for 2 hours to obtain an alumina powder with a D50 of 12.99 μm.
[0081] (2) Select ethanol as the extractant, and the volume ratio of the extractant to the alumina dispersion is 1:3. Add 200 mL of ethanol to a container, add 600 mL of alumina dispersion prepared by mixing the pretreated alumina powder with a solid content of 30% to the container, and place it on a constant temperature magnetic stirrer and stir at 30°C for 60 minutes for use.
[0082] The stirred alumina mixture was added to a centrifuge test tube and placed in a centrifuge at 150 rpm for 30 minutes. After centrifugation, the alumina mixture in the centrifuge test tube was taken out and added to a separatory funnel for separation. After standing and stratification, the lower layer of alumina slurry was flowed out from the lower mouth of the separatory funnel into a beaker to obtain alumina slurry.
[0083] (3) Add the alumina slurry into a horizontal sand mill for grinding, using alumina beads as the grinding medium, with a diameter of 0.3-0.6 mm, a ball-to-material ratio of 5:1, grinding for 6 hours, and a grinding speed of 2000 rpm; the ground ultrafine alumina slurry is dried at 110° C. for 3 hours to obtain ultrafine low-sodium, low-silicon alumina.
[0084] X-ray fluorescence spectrometry (XRF) was used to test the content of each element, and the test results were as follows: the content of aluminum oxide in the product was 99.7%, the content of sodium was 0.18%, the content of silicon was 0.08%, and the rest were other impurities.
[0085] The particle size of the powder was measured using a laser particle size analyzer, and the average particle size was 1.553 μm.
[0086] Comparative Example 3
[0087] This comparative example relates to the preparation of an ultrafine alumina powder. The difference from Example 1 is that the extractant is n-hexane, and the volume ratio of the extractant to the alumina dispersion is 1:5. Specifically:
[0088] (1) A certain amount of industrial alumina (D50 of 31.83 μm) was spread in an oven and dried at 100-110°C for 1-2 hours to obtain a dried alumina sample. The dried alumina was ball-milled with a ball-to-material ratio of 6:1. The ball-milling medium was alumina balls with diameters of 10 mm, 8 mm, 5 mm, and 3 mm in a mass ratio of 1:2:3:4. The alumina powder was first ball-milled at 500 rpm for 2 hours and then at 400 rpm for 2 hours to obtain an alumina powder with a D50 of 12.99 μm.
[0089] (2) Select n-hexane as the extractant, and the volume ratio of the extractant to the alumina dispersion is 1:5. Add 150 mL of n-hexane to a container, add 750 mL of alumina dispersion prepared by mixing the pretreated alumina powder with a solid content of 30% to the container, and place it on a constant temperature magnetic stirrer. Stir at 30°C for 60 minutes and set aside.
[0090] The stirred alumina mixture was added to a centrifuge test tube and placed in a centrifuge at 150 rpm for 30 minutes. After centrifugation, the alumina mixture in the centrifuge test tube was taken out and added to a separatory funnel for separation. After standing and stratification, the lower layer of alumina slurry was flowed out from the lower mouth of the separatory funnel into a beaker to obtain alumina slurry.
[0091] (3) Add the alumina slurry into a horizontal sand mill for grinding, using alumina beads as the grinding medium, with a diameter of 0.3-0.6 mm, a ball-to-material ratio of 5:1, grinding for 6 hours, and a grinding speed of 2000 rpm; the ground ultrafine alumina slurry is dried at 110° C. for 3 hours to obtain ultrafine low-sodium, low-silicon alumina.
[0092] X-ray fluorescence spectrometry (XRF) was used to test the content of each element, and the test results were as follows: the content of aluminum oxide in the product was 99.72%, the content of sodium was 0.22%, the content of silicon was 0.05%, and the rest were other impurities.
[0093] The particle size of the powder was measured using a laser particle size analyzer, and the average particle size was 1.863 μm.
[0094] The content of each component in the ultrafine alumina powder prepared in Examples 1-3 and Comparative Examples 1-3 and the average particle size at different stages are shown in Table 1 below:
[0095] Table 1
[0096]
[0097] As can be seen from Table 1, the present invention uses an extractant prepared by mixing ethanol and n-hexane in a certain volume ratio to extract the ball-milled industrial alumina, which can effectively reduce the content of sodium and silicon impurities in the industrial alumina, so that the purity of the prepared alumina is as high as 99.9% or more, and obtain ultrafine low-sodium and low-silicon alumina powder.
[0098] The above-described embodiments are merely preferred examples for the purpose of fully illustrating the present invention, and the scope of protection of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are within the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
Claims
1. A method for preparing ultrafine low sodium and low silicon alumina powder, characterized in that: The following steps are involved: (1) ball-milling industrial alumina to obtain alumina powder; (2) dispersing the alumina powder prepared in step (1) in water to obtain an alumina dispersion; mixing and stirring the alumina dispersion with an extractant to obtain an alumina mixed solution; centrifuging and separating the alumina mixed solution to obtain an alumina slurry; the extractant is a mixed solvent of ethanol and n-hexane; (3) Grinding the alumina slurry and drying it to obtain the ultrafine low-sodium and low-silicon alumina powder.
2. The preparation method according to claim 1, characterized in that: In step (1), the industrial alumina satisfies at least one of the following characteristics: (1) The industrial alumina is a block or granular solid; (2) The D50 of the industrial alumina is 30-40 μm; (3) The industrial alumina has a purity of ≦99.7%, a silicon content of ≧0.05%, and a sodium content of ≧0.17%.
3. The preparation method according to claim 1, characterized in that: In step (1), in the ball milling step: the ball milling medium is alumina balls, the ball-to-material ratio is 5-7:1, the ball milling speed is 400-500 rpm, and the ball milling time is 3-6 hours; The ball milling medium is obtained by mixing alumina balls with diameters of 10 mm, 8 mm, 5 mm, and 3 mm in a mass ratio of 1:2:3:4; The particle size of the aluminum oxide powder is 1-2 μm.
4. The preparation method according to claim 1, characterized in that: In step (2), the volume ratio of ethanol to n-hexane in the extractant is 1:(3-5); The solid content of the aluminum oxide dispersion is 20%-40%; The volume ratio of the alumina dispersion to the extractant is (1-3):
1.
5. The preparation method according to claim 1, characterized in that: In step (2), the mixing temperature is 20-50°C, and the mixing time is 30-60min; The centrifugal speed is 100-200 rpm, and the time is 15 min-1 h; The step of separating the liquids is specifically as follows: the alumina mixed liquid after centrifugal treatment is allowed to stand for treatment, and after standing and stratifying, the alumina slurry in the lower layer is obtained.
6. The preparation method according to claim 1, characterized in that: In step (3), in the grinding step: the grinding medium is alumina beads, the ball-to-material ratio is 5-10:1, the grinding speed is 1500-3000 rpm, and the grinding time is 4-6 hours; The diameter of the alumina beads is 0.3-0.6 mm.
7. The preparation method according to claim 1, characterized in that: In step (3), the drying temperature is 100-120° C. and the drying time is 2-4 hours.
8. An ultrafine low sodium and low silicon alumina powder prepared by the preparation method according to any one of claims 1 to 7.
9. The ultrafine low sodium and low silicon alumina powder according to claim 8, characterized in that: The average particle size of the ultrafine low sodium and low silicon alumina powder is 200-500nm; The ultrafine low-sodium and low-silicon alumina powder has an alumina content of ≥99.9%, a sodium content of ≤0.05%, and a silicon content of <0.05%.
10. A lithium battery separator, characterized in that: It comprises a base film and a coating arranged on at least one side of the base film along the thickness direction; the coating comprises the ultrafine low-sodium and low-silicon alumina powder according to claim 8 or 9.