Preparation method of ternary positive electrode material

Through multiple sintering processes and molar ratio control methods, the ternary positive electrode material LiNixCoyMnzO2 was prepared, which solved the problems of high cost and poor particle uniformity of the positive electrode material of high nickel lithium-ion batteries, and achieved improvement of particle uniformity and electrochemical performance. .

CN119080078AInactive Publication Date: 2024-12-06HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411009224.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing high-nickel lithium-ion battery positive electrode materials are costly and have poor particle uniformity in production, especially when using lithium hydroxide process, the particle uniformity is poor when using lithium carbonate process, resulting in the urgent need for an improved particle uniformity. preparation method.

Method used

The ternary positive electrode material LiNixCoyMnzO2 was prepared by multiple sintering. Partially lithiated in the low-temperature section through primary sintering, secondary sintering decomposes CoOOH and coat it on the surface. The third sintering decomposes H3BO3 and coat it with secondary sintering, combining the control of LiOH and The molar ratio and sintering conditions of Li2CO3 improve particle uniformity and electrochemical properties.

Benefits of technology

The particle uniformity and electrochemical performance of the ternary positive electrode material are improved, production costs are reduced, and uniformity of high-nickel NCM materials and excellent battery capacity, first-effect and cycle stability are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080078A_ABST
    Figure CN119080078A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a ternary positive electrode material, and relates to the technical field of lithium ion batteries. A preparation method of a ternary positive electrode material comprises the following steps: S1, mixing NixCoyMn (1-x-y) (OH) 2, Li2CO3, LiOH and Nb2O5 to obtain a mixture A, and carrying out primary sintering on the mixture A to obtain a material B; s2, crushing the material B, mixing the crushed material B with CoOOH to obtain a mixture C, and carrying out secondary sintering on the mixture C to obtain a mixture D; and S3, sieving the mixture D, mixing the sieved mixture D with H3BO3 to obtain a mixture E, and sintering the mixture E for the third time to obtain the ternary positive electrode material LiNixCoyMnzO2. The ternary positive electrode material prepared by the method provided by the invention has uniform particles and excellent electrochemical performance, and the assembled battery has excellent battery capacity, initial efficiency and cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a ternary positive electrode material. Background Art

[0002] With the progress of society and the development of technology, human beings have an increasing demand for energy. As an emerging energy storage technology, lithium batteries are not only widely used in mobile communications, electric vehicles and other fields around the world, but are also gradually becoming a hot spot in the international energy field. As one of the important components of lithium-ion batteries, cathode materials play a key role in battery performance.

[0003] Common positive electrode materials include LiCoO2, LiNiO2, LiMnO2 and LiNi x Co y Mn 1-y-z O2(NCM), NCM has the advantages of low cost, large discharge capacity and good cycle performance compared to other positive electrode materials. The lithium source of NCM in production mainly comes from lithium hydroxide (LiOH) or lithium carbonate (Li2CO3), but the cost of producing high-nickel NCM using the LiOH process is too high, and the high-nickel NCM produced using the Li2CO3 process has poor particle uniformity. Therefore, it is urgent to develop a preparation method for ternary positive electrode materials to improve particle uniformity, which is of great significance for the widespread application of positive electrode materials. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a method for preparing a ternary positive electrode material.

[0005] A method for preparing a ternary positive electrode material proposed by the present invention comprises the following steps:

[0006] S1. Ni x Co y Mn (1-x-y) (OH)2, Li2CO3, LiOH and Nb2O5 are mixed to obtain a mixture A, and the mixture A is sintered once to obtain a material B;

[0007] S2, crushing material B and mixing it with CoOOH to obtain a mixture C, and performing secondary sintering on the mixture C to obtain a mixture D;

[0008] S3, after sieving the mixture D, mix it with H3BO3 to obtain a mixture E, and sinter the mixture E three times to obtain a ternary positive electrode material LiNi x Co y Mn z O2.

[0009] The present invention obtains the ternary positive electrode material LiNi by multiple sintering processes x Co y Mn z O2 helps to improve the particle uniformity of the ternary cathode material. x Co y Mn (1-x-y) (OH)2 undergoes partial lithiation in the low temperature section and then fully completes lithiation in the high temperature section. At the same time, the Nb element can be doped into the lattice of the nickel-cobalt-manganese ternary positive electrode material; the secondary sintering is to decompose CoOOH into Co2O3 and coat it on the surface of the nickel-cobalt-manganese ternary positive electrode material; the tertiary sintering is to decompose H3BO3 into B2O3 and coat it on the nickel-cobalt-manganese ternary positive electrode material for the second time.

[0010] Preferably, in the S1, the molar ratio of LiOH to Li2CO3 is (1-10):100.

[0011] The present invention helps to improve the uniformity of particles and control costs by controlling the molar ratio of LiOH and Li2CO3 within a certain range. Adding a small amount of LiOH during a sintering process can improve the uniformity of particles of high-nickel NCM materials. When LiOH exists in the sintering system, nickel-cobalt-manganese hydroxide will begin to undergo lithiation reaction in the low temperature section (200-240°C); if LiOH does not exist, the lithiation reaction will occur in the high temperature section. First, the high temperature section lasts longer, and the energy consumed is higher; second, long-term high-temperature calcination will over-consume lithium source, and the lithium source will burn too much, increasing costs; third, long-term high-temperature calcination will cause the grains to grow unevenly, resulting in uneven particles. The present invention prepares high-nickel NCM materials by using Li2CO3 and a small amount of LiOH, so that it undergoes lithiation reaction in the low temperature section, which not only improves the uniformity of particles, but also effectively controls production costs.

[0012] Preferably, in the S1, Ni x Co y Mn (1-x-y) The value of x in (OH)2 is 0.6-0.8, and the value of y is 0.05-0.20.

[0013] By limiting Ni x Co y Mn (1-x-y) The values ​​of x and y in (OH)2 being within a certain range helps to ensure that the prepared ternary positive electrode material is a high-nickel material, making the preparation method of the present invention more advantageous in improving particle uniformity and material performance.

[0014] Preferably, in S1, the mixing speed is 750-860 r / min, and the mixing time is 10-40 min.

[0015] Mixing speed and time within a certain range can help improve the uniformity of dispersion between materials.

[0016] Preferably, in S1, the primary sintering comprises heating the temperature to 870-950° C. at a heating rate of 1-5° C. / min and keeping the temperature for 10-20 hours.

[0017] The primary sintering temperature and time within a certain range will help ensure Ni x Co y Mn (1-x-y) Full lithiation of (OH)2 and growth of primary particles.

[0018] Preferably, in the S1, Nb2O5, Ni x Co y Mn (1-x-y) The mass ratio of (OH)2 is 0.05%-0.25%.

[0019] Preferably, in the S2, the mass ratio of CoOOH to material B is 0.03%-1%.

[0020] Preferably, in the S3, the mass ratio of H3BO3 to mixture D is 0.04%-0.35%.

[0021] The synergistic effect of controlling the addition of a certain amount of Nb2O5, CoOOH, and H3BO3 helps to improve the electrochemical performance. The Nb, Co, and B elements provided by Nb2O5, CoOOH, and H3BO3 can reduce the side reactions between the material and the electrolyte, inhibit the dissolution of metal ions, and prevent the impedance from increasing during the charge and discharge process, thereby improving the cycle performance of the material. Combined with the good uniformity of the particles, it has excellent electrical properties after being made into a battery. However, adding too much Nb, Co, and B elements will cause unnecessary waste, and there will also be side effects. For example, the thicker the coating layer, the more lithium ion transmission paths will increase, and the polarization will increase; while adding less will not achieve the expected effect. For example, if there is less coating, it will cause uneven coating and fail to isolate the electrolyte and support the structure.

[0022] Preferably, in S2, the mixing speed is 800-870 r / min, and the mixing time is 10-40 min.

[0023] Mixing speed and time within a certain range can help improve the uniformity of dispersion between materials.

[0024] Preferably, in S2, the secondary sintering comprises heating the temperature to 620-700°C at a heating rate of 1-5°C / min and keeping the temperature for 4-7h.

[0025] The secondary sintering temperature and time within a certain range are helpful to ensure that CoOOH is fully decomposed by heat and can be coated on the surface of the ternary material particles.

[0026] Preferably, in S3, the mixing speed is 720-880 r / min, and the mixing time is 10-40 min.

[0027] Mixing speed and time within a certain range can help improve the uniformity of dispersion between materials.

[0028] Preferably, in S3, the three sinterings include heating the temperature to 260-385°C at a heating rate of 1-5°C / min and keeping the temperature for 2-6h.

[0029] The tertiary sintering temperature and time within a certain range are helpful to ensure that H3BO3 is fully decomposed by heat and can be coated on the surface of the ternary material particles.

[0030] The present invention also provides a ternary positive electrode material prepared by the above method.

[0031] The beneficial effects of the present invention are:

[0032] The present invention uses a step-by-step sintering method to sequentially complete the bulk doping of Nb elements and the double-layer coating of Co2O3 and B2O3, which can stabilize the layered structure during the charge and discharge process and improve the electrochemical performance. The preparation method of the ternary positive electrode material provided by the present invention is simple, improves the uniformity of particles, has abundant raw materials, low energy consumption, safe and reliable production process, low production cost, and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The scanning electron microscope images of Example 1(a) and Comparative Example 1(b) proposed by the present invention. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is described in detail through specific embodiments.

[0035] Unless otherwise specified, the materials, reagents, etc. used in the following examples and comparative examples can be obtained from commercial sources.

[0036] Example 1

[0037] A method for preparing a ternary positive electrode material comprises the following steps:

[0038] S1, 300g Ni x Co y Mn (1-x-y)(OH)2, 122.44g Li2CO3, 1.42g LiOH, 0.215g Nb2O5 are mixed to obtain mixture A, and mixture A is sintered once to obtain material B; the mixing speed is 820r / min, and the mixing time is 30min; the primary sintering is carried out at a heating rate of 2℃ / min to 910℃ and kept warm for 15h;

[0039] S2. After crushing material B, 120 g of material B was mixed with 1.12 g of CoOOH to obtain a mixture C, and the mixture C was subjected to secondary sintering to obtain a mixture D; the mixing speed was 820 r / min, and the mixing time was 20 min; the secondary sintering was performed by heating the temperature to 620 ° C at a heating rate of 2 ° C / min and keeping the temperature for 5 h;

[0040] S3, after sieving the mixture D, it was mixed with 0.343g H3BO3 to obtain the mixture E, and the mixture E was sintered three times, and the obtained mixture was sieved to obtain the ternary positive electrode material LiNi x Co y Mn z O2; the mixing speed is 780r / min, and the mixing time is 30min; the third sintering is to increase the temperature to 380℃ at a heating rate of 2℃ / min and keep it warm for 5h.

[0041] Example 2

[0042] A method for preparing a ternary positive electrode material comprises the following steps:

[0043] S1, 300g Ni x Co y Mn (1-x-y) (OH)2, 123.06g Li2CO3, 0.71g LiOH, 0.215g Nb2O5 are mixed to obtain mixture A, and mixture A is sintered once to obtain material B; the mixing speed is 820r / min, and the mixing time is 30min; the primary sintering is carried out at a heating rate of 2℃ / min to 910℃ and kept warm for 15h;

[0044] S2. After crushing material B, 120 g of material B was mixed with 1.12 g of CoOOH to obtain a mixture C, and the mixture C was subjected to secondary sintering to obtain a mixture D; the mixing speed was 820 r / min, and the mixing time was 20 min; the secondary sintering was performed by heating the temperature to 620 ° C at a heating rate of 2 ° C / min and keeping the temperature for 5 h;

[0045] S3, after sieving the mixture D, it was mixed with 0.343g H3BO3 to obtain the mixture E, and the mixture E was sintered three times, and the obtained mixture was sieved to obtain the ternary positive electrode material LiNi x Coy Mn z O2; the mixing speed is 780r / min, and the mixing time is 30min; the third sintering is to increase the temperature to 380℃ at a heating rate of 2℃ / min and keep it warm for 5h.

[0046] Example 3

[0047] A method for preparing a ternary positive electrode material comprises the following steps:

[0048] S1, 300g Ni x Co y Mn (1-x-y) (OH)2, 121.82g Li2CO3, 2.13g LiOH, 0.215g Nb2O5 are mixed to obtain mixture A, and mixture A is sintered once to obtain material B; the mixing speed is 820r / min, and the mixing time is 30min; the primary sintering is carried out at a heating rate of 2℃ / min to 910℃ and kept warm for 15h;

[0049] S2. After crushing material B, 120 g of material B was mixed with 1.12 g of CoOOH to obtain a mixture C, and the mixture C was subjected to secondary sintering to obtain a mixture D; the mixing speed was 820 r / min, and the mixing time was 20 min; the secondary sintering was performed by heating the temperature to 620 ° C at a heating rate of 2 ° C / min and keeping the temperature for 5 h;

[0050] S3, after sieving the mixture D, it was mixed with 0.343g H3BO3 to obtain the mixture E, and the mixture E was sintered three times, and the obtained mixture was sieved to obtain the ternary positive electrode material LiNi x Co y Mn z O2; the mixing speed is 780r / min, and the mixing time is 30min; the third sintering is to increase the temperature to 380℃ at a heating rate of 2℃ / min and keep it warm for 5h.

[0051] Comparative Example 1

[0052] The only difference between this comparative example and Example 1 is that the mass of Li2CO3 in S1 is 123.77 g, and LiOH is no longer added; the other steps are the same as those in Example 1.

[0053] Comparative Example 2

[0054] The difference between this comparative example and Example 1 is that Nb2O5 is not added to S1; the other steps are the same as those in Example 1.

[0055] Comparative Example 3

[0056] A method for preparing a ternary positive electrode material comprises the following steps:

[0057] S1, 300g Ni x Co y Mn (1-x-y) (OH)2, 122.44g Li2CO3, 1.42g LiOH, 0.215g Nb2O5 are mixed to obtain mixture A, and mixture A is sintered once to obtain material B; the mixing speed is 820r / min, and the mixing time is 30min; the primary sintering is carried out at a heating rate of 2℃ / min to 910℃ and kept warm for 15h;

[0058] S2. After crushing material B, 120 g of material B was mixed with 0.343 g of H3BO3 to obtain a mixture E. The mixture E was sintered three times, and the material was sieved to obtain a ternary positive electrode material LiNi x Co y Mn z O2; the mixing speed is 780r / min, and the mixing time is 30min; the third sintering is to increase the temperature to 380℃ at a heating rate of 2℃ / min and keep it warm for 5h.

[0059] Comparative Example 4

[0060] A method for preparing a ternary positive electrode material comprises the following steps:

[0061] S1, 300g Ni x Co y Mn (1-x-y) (OH)2, 122.44g Li2CO3, 1.42g LiOH, 0.215g Nb2O5 are mixed to obtain mixture A, and mixture A is sintered once to obtain material B; the mixing speed is 820r / min, and the mixing time is 30min; the primary sintering is carried out at a heating rate of 2℃ / min to 910℃ and kept warm for 15h;

[0062] S2, after crushing material B, take 120g material B and 1.12g CoOOH to mix to obtain mixture C, and perform secondary sintering on mixture C to obtain mixture D; after discharging, sieve to obtain ternary positive electrode material LiNi x Co y Mn z O2; the mixing speed is 820r / min, and the mixing time is 20min; the secondary sintering is to heat up to 620℃ at a heating rate of 2℃ / min and keep it warm for 5h.

[0063] The ternary positive electrode material prepared in the above embodiments and comparative examples is used as the positive electrode material, the lithium sheet is used as the negative electrode, the superconducting carbon black SuperP is used as the conductive agent, polyvinylidene fluoride (PVDF) is used as the binder, and N-methylpyrrolidone (NMP) is used as the solvent. The single crystal material and the superconducting carbon black SuperP are ground and then added to a solution of N-methylpyrrolidone dissolved with polyvinylidene fluoride. The mass ratio of the positive electrode material, SuperP and PVDF is 8:1:1. After stirring for 2 hours, the mixture is coated on the surface of a 20μm thick aluminum foil and then vacuum dried at 110°C for 20 hours. The dried pole piece is rolled, sliced, and weighed, and then assembled into a CR2016 button cell with a metal lithium sheet and a diaphragm prepared by a wet process in an argon atmosphere glove box. The electrolyte is 1.0mol / LLiPF6 / EC+DEC+EMC. The assembled button cell is subjected to an electrochemical performance test, and the test voltage range is 2.8-4.3V. Detailed data are shown in Table 1.

[0064] Table 1

[0065]

[0066] From the electrochemical data in Table 1, it can be seen that the ternary cathode material prepared by the present invention is assembled into a battery, which has a high 0.2C first discharge gram capacity, first coulomb efficiency, 1C discharge gram capacity and 50-week capacity retention rate, indicating that the ternary cathode material prepared by the present invention has excellent electrochemical performance. From the data in Table 1 and Figure 1 It can be seen that the addition of LiOH will improve the uniformity of the material particles. The synergistic effect of Li2CO3 and LiOH not only improves the uniformity of the particles but also improves the battery capacity, first efficiency and cycle stability. Compared with Comparative Example 2, it can be seen from Examples 1-3 that Nb doping will improve the stability of the material structure, thereby improving the electrochemical performance of the material. Compared with Comparative Examples 3 and 4, it can be seen that the double-layer coating effect is better in Examples 1-3, and it has more advantages in reducing electrolyte contact and stabilizing the structure.

[0067] In summary, the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided by the present invention has uniform particles and excellent electrochemical properties, and the battery assembled from the ternary positive electrode material has excellent battery capacity, first efficiency and cycle stability.

[0068] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a ternary positive electrode material, characterized in that: The following steps are involved: S1. Ni x Co y Mn (1-x-y) (OH)2, Li2CO3, LiOH and Nb2O5 are mixed to obtain a mixture A, and the mixture A is sintered once to obtain a material B; S2, crushing material B and mixing it with CoOOH to obtain a mixture C, and performing secondary sintering on the mixture C to obtain a mixture D; S3, after sieving the mixture D, mix it with H3BO3 to obtain a mixture E, and sinter the mixture E three times to obtain a ternary positive electrode material LiNi x Co y Mn z O2.

2. The method according to claim 1, characterized in that In the S1, the molar ratio of LiOH and Li2CO3 is (1-10):

100.

3. The method according to claim 1, characterized in that In the S1, the mixing speed is 750-860r / min, and the mixing time is 10-40min; in the S2, the mixing speed is 800-870r / min, and the mixing time is 10-40min; in the S3, the mixing speed is 720-880r / min, and the mixing time is 10-40min.

4. The method according to claim 1, characterized in that In the above-mentioned S1, the primary sintering includes heating the temperature to 870-950°C at a heating rate of 1-5°C / min and keeping the temperature for 10-20h.

5. The method according to claim 1, characterized in that: In the S2, the secondary sintering includes heating the temperature to 620-700°C at a heating rate of 1-5°C / min and keeping the temperature for 4-7h.

6. The method according to claim 1, characterized in that In the S3, the three sinterings include heating to 260-385°C at a heating rate of 1-5°C / min and keeping the temperature for 2-6h.

7. The method according to claim 1, characterized in that In the S1, Nb2O5, Ni x Co y Mn (1-x-y) The mass ratio of (OH)2 is 0.05%-0.25%; in the S2, the mass ratio of CoOOH and material B is 0.03%-1%; in the S3, the mass ratio of H3BO3 and mixture D is 0.04%-0.35%.

8. A ternary positive electrode material, characterized in that: The method is prepared by any one of claims 1 to 7.

Citation Information

Patent Citations

  • Method for preparing high-nickel cathode material for lithium secondary battery

    CN110137488A

  • Micron-sized lithium ion battery positive electrode material and preparation method thereof

    CN114162879A

  • High-voltage ternary positive electrode material and preparation method thereof

    CN115911300A

  • High-nickel positive electrode material as well as preparation method and application thereof

    CN116239159A

  • Positive electrode material, preparation method thereof and lithium ion battery

    CN117613230A