Geopolymer grouting material as well as preparation method and application thereof

By using geopolymer grouting materials prepared by fly ash, cement, waterproofing agents and alkaline exciters, the problems of high construction costs and insufficient physical strength in the prior art are solved, and efficient sealing and pollutant removal are achieved. It reduces carbon emissions and heavy metal leaching toxicity, and is suitable for the treatment of acidic groundwater in coal mines.

CN119080458APending Publication Date: 2024-12-06CHINA UNIV OF MINING & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411208313.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Among the existing coal mine groundwater pollution repair technologies, cement slurry has high construction cost and poor corrosion resistance. The physical strength of fly slurry is too low, the modification process is complex and the cost is high, making it difficult to effectively seal acid mine water and remove pollutants.

Method used

Using geopolymer grouting materials composed of fly ash, cement, waterproofing agent and alkaline exciter, are prepared through specific mass ratios and process flows to form grouting materials with high compressive strength, which can quickly seal groundwater flow. and remove contaminants.

Benefits of technology

It reduces cement usage, reduces carbon emissions and raw material costs, improves the corrosion resistance and pollutant removal capabilities of the materials, achieves rapid sealing and stabilization of pollutants, reduces the toxicity of heavy metal leaching, and is suitable for the treatment of acidic groundwater in coal mines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080458A_ABST
    Figure CN119080458A_ABST
Patent Text Reader

Abstract

The invention provides a geopolymer grouting material as well as a preparation method and application thereof, and belongs to the technical field of wastewater treatment. The geopolymer grouting material is composed of slurry and an alkaline activator. The slurry is composed of fly ash, cement, a waterproof agent and water; the mass ratio of the fly ash to the cement is (6-9): (1-4); the addition amount of the waterproof agent is 0.4-0.7% of the total mass of the fly ash and the cement; the addition amount of the water is 0.8-1% of the total mass of the fly ash and the cement; the mass ratio of the alkaline activator to the fly ash is (11-20): (60-90). The geopolymer grouting material provided by the invention is simple to prepare and high in compressive strength, can quickly block an underground water flow channel, and also can react with polluted mine water to remove pollutants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment, and in particular to a geopolymer grouting material and a preparation method and application thereof. Background Art

[0002] Sulfur in coal mainly exists in two forms: organic sulfur and inorganic sulfur. There is also trace elemental sulfur in a free state. The collective name of inorganic sulfur, organic sulfur and elemental sulfur in coal is total sulfur. Among them, organic sulfur refers to sulfur formed by combining with organic matter in coal, which is difficult to remove from coal and accounts for more than 70% of the total sulfur; while inorganic sulfur refers to sulfur in the form of minerals, which can be removed by physical and chemical methods, accounting for about 30% of the total sulfur. Coal has a high sulfur content. After the ore seam is exposed due to mining, high-sulfur coal will react in the coal seam to produce high-sulfate acid mine water that pollutes groundwater, deeply endangering the ecological environment and human health and safety.

[0003] Grouting treatment, as an in-situ injection repair method, is currently a hot technology in the field of mine water pollution remediation. Using grouting materials to fill the cracks in the surrounding rock of the mine or fill the coal field goaf can not only effectively support the coal seam and block the contaminated underground water, but also inhibit the oxidation reaction of the coal seam, block the migration of pollutants and purify the groundwater.

[0004] In the current coal mine groundwater pollution remediation sites, cement slurry or fly ash solid waste slurry is mostly used for in-situ grouting and sealing treatment. The former has high construction costs, poor corrosion resistance and large carbon emissions during cement production, while the latter has too low physical strength, poor pollution reduction ability, complex modification process and too high modification cost. Summary of the invention

[0005] In view of the above problems, the present invention provides a geopolymer grouting material and a preparation method and application thereof. The geopolymer grouting material provided by the present invention is simple to prepare, has high compressive strength, and less heavy metal leaching. It can quickly block underground water flow channels and can also react with contaminated mine water to remove pollutants.

[0006] The first object of the present invention is to provide a geopolymer grouting material, which consists of a slurry and an alkaline activator;

[0007] The slurry is composed of fly ash, cement, waterproofing agent and water. Fly ash and cement are used to block the water inrush of acid mines and remove pollution. The waterproofing agent is used to increase the water injection property of the surface of the grouting material.

[0008] The mass ratio of fly ash and cement is 6-9:1-4; for example, the mass ratio of fly ash and cement is 6:4, 6.5:3.5, 7:3, 7.5:2.5, 8:2, 8.5:1.5, 9:1, etc., but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable, which will not be elaborated here.

[0009] The amount of waterproofing agent added is 0.4% to 0.7% of the total mass of fly ash and cement; for example, the amount of waterproofing agent added is 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7% and the like of the total mass of fly ash and cement, but is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable, so they will not be repeated here.

[0010] The amount of water added is 0.8 to 1 of the total mass of fly ash and cement; for example, the amount of water added is 0.8, 0.85, 0.9, 0.95, 1, etc. of the total mass of fly ash and cement, but is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable, so they will not be repeated here.

[0011] The mass ratio of alkaline activator to fly ash is 11-20:60-90; for example, the mass ratio of alkaline activator to fly ash is 11:60, 15:60, 20:60, 11:70, 15:70, 20:70, 11:80, 15:80, 20:80, 11:90, 15:90, 20:90, etc., but is not limited to the listed values, other values ​​not listed within the above numerical range are also applicable, which will not be repeated here.

[0012] In a preferred embodiment of the present invention, the mass ratio of fly ash to cement is 3:2.

[0013] In a preferred embodiment of the present invention, the added amount of the waterproofing agent is 0.7% of the total mass of the fly ash and cement.

[0014] In a preferred embodiment of the present invention, the mass ratio of the alkaline activator to the fly ash is 1:4.

[0015] In a preferred embodiment of the present invention, the alkaline activator is water glass, and the modulus of the water glass is 3.11-3.40 and the density is 1-5 g / ml.

[0016] In a preferred embodiment of the present invention, the waterproofing agent is sodium methyl silicate or isobutyl triethoxy silane.

[0017] In a preferred embodiment of the present invention, the specific surface area of ​​cement is 0.1m 2 / g~20m 2 / g;

[0018] The residue of fly ash on a 45μm square hole sieve is 1% to 30%, and the loss on ignition is 1% to 10%.

[0019] A second object of the present invention is to provide a method for preparing the above-mentioned geopolymer grouting material, comprising the following steps:

[0020] Weigh fly ash and cement according to the mass ratio of fly ash to cement of 6-9:1-4; weigh the waterproofing agent according to the addition amount of the waterproofing agent of 0.4%-0.7% of the total mass of fly ash and cement; weigh the water according to the addition amount of water of 0.8-1 of the total mass of fly ash and cement;

[0021] Weigh the alkaline activator according to the mass ratio of alkaline activator to fly ash of 11-20:60-90;

[0022] The fly ash, cement and waterproofing agent are mixed once to obtain a mixed material;

[0023] The mixed material is mixed with water for a second time to obtain a mixed slurry;

[0024] The mixed slurry is mixed with the alkaline activator three times to obtain the geopolymer grouting material.

[0025] In a preferred embodiment of the present invention, the stirring time of the first mixing is 3 min to 5 min; and the stirring time of the second mixing is 5 min to 8 min.

[0026] The third object of the present invention is to provide the application of the above-mentioned geopolymer grouting material in filling the surrounding rock cracks of mines or the goaf of coal fields, and the slurry and alkaline activator in the geopolymer grouting material are injected into the formation by the double liquid grouting method.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention combines fly ash and cement, and the mass ratio of fly ash to cement is 6-9:1-4. On the one hand, fly ash replaces part of cement, reducing the amount of cement used, thereby reducing carbon emissions and greatly reducing the cost of raw materials. On the other hand, fly ash is mainly composed of compounds such as silicon dioxide, aluminum oxide and iron oxide. The mass ratio of alkaline activator to fly ash is 11-20:60-90. Fly ash can be activated in the alkaline environment provided by cement hydration and alkaline activator hydrolysis, and a geopolymerization process occurs to generate gel products such as hydrated calcium silicate and hydrated calcium aluminate, thereby enhancing its ability to adsorb and remove pollutants. Cement can ensure the physical strength of the slurry after solidification, support the formation and improve the resistance to water flow impact, and it has the function of solidifying and stabilizing pollutants. Adding an alkaline activator can ensure the rapid setting of the slurry to achieve the purpose of rapid solidification and blocking the water flow channel. Its hydrolysis can provide an alkaline environment to neutralize acidic groundwater and promote the geopolymerization reaction and cement hydration reaction process. Adding 0.4% to 0.7% of the total mass of fly ash and cement as a waterproofing agent can enhance the corrosion resistance of the slurry after solidification. It can also promote the cement hydration reaction process and improve the physical strength of the material.

[0029] (2) The grouting material prepared by the present invention can not only meet the requirements of the solidification strength of the formation grouting material, but also can quickly block the groundwater flow channel after the in-situ grouting construction to reduce the outburst of acidic groundwater in coal mines, and can also react with contaminated mine water through adsorption, solidification and stabilization to remove pollutants such as heavy metals and sulfates, thereby reducing the harm of acidic groundwater in coal mines to the surrounding environment and human health and safety.

[0030] (3) The grouting material prepared by the present invention has lower heavy metal leaching toxicity, is environmentally friendly, and effectively utilizes fly ash, a large coal-based solid waste, without secondary pollution.

[0031] (4) The material formula of the present invention is simple and easy to obtain locally; the preparation method is simple and easy to implement; the solid waste ratio is high, environmentally friendly and low-cost; the proportion and amount of raw materials can be adjusted according to the technical requirements of different engineering sites, and can be used for the treatment of mine water pollution in operating or closed coal mines. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is the compressive strength of the grouting materials prepared in Examples 1-6 and Comparative Examples 1-4.

[0033] Figure 2 This is the X-ray diffraction analysis diagram of different grouting materials after acid mine water curing. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The present invention uses fly ash and cement in combination. Fly ash, as a kind of coal-based solid waste, is easy to obtain near the coal mining area, has low cost, and has porosity and large specific surface area, and can effectively adsorb heavy metal pollutants, etc. A geopolymerization reaction can occur through an alkali-activated fly ash modification method, further improving its adsorption performance. Cement can solidify and stabilize heavy metal pollutants, etc., and it has a certain effect of neutralizing acidity. In summary, the present invention uses fly ash as the main raw material and combines cement and the like as a slurry material to inject in situ into the coal mine stratum containing polluted water bodies, which can not only effectively block the acid mine water gushing and remove pollutants, but also achieve the goal of treating waste with waste and reducing carbon emissions. In addition, the present invention additionally adds a waterproofing agent such as sodium methyl silicate, which can generate a layer of insoluble resin film on the surface of the material through chemical reaction, increase the hydrophobicity of the surface of the material, and can also improve the concrete structure and increase the density. And the addition of sodium methyl silicate can improve the structural stability and strength of the fly ash-cement-based geopolymer test block under the condition of acid mine water immersion.

[0036] When the modulus of water glass is small, the silica content is low, the gel time is long, and the strength of the grouting material is low; when the modulus of water glass is large, the silica content is high, the gel time is short, and the strength of the grouting material is high. Too large or too small a modulus of water glass is not conducive to grouting. Therefore, when grouting, it is generally more appropriate to require the modulus of water glass to be between 2.4 and 3.4.

[0037] The high silicon and aluminum content of fly ash is conducive to the formation of geopolymers. The test results of the fly ash used in the present invention are shown in Table 1.

[0038] Table 1 Test report of primary fly ash used in the present invention

[0039]

[0040] Cement powder: The cement powder used in the present invention is PO 42.5 cement, with a specific surface area of ​​3.58m 2 The cement test report used in the present invention is shown in Table 2.

[0041] Table 2 Test report of PO 42.5 cement used in the present invention

[0042]

[0043]

[0044] Example 1

[0045] The geopolymer grouting material provided in this embodiment includes the following components in parts by weight: 60 parts of fly ash, 40 parts of cement, 15 parts of alkaline activator water glass, 0.7 parts of waterproofing agent sodium methyl silicate, and 80 parts of water.

[0046] The fly ash used in this example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0047] Waterproofing agent: sodium methyl silicate, white solid powder, solid content ≥98%.

[0048] In this embodiment, the water-cement ratio is 0.8, that is, water accounts for 0.8 of the total mass of cement and fly ash;

[0049] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0050] The ash ratio is 0.7%, that is, sodium methyl silicate accounts for 0.7% of the total mass of cement and fly ash.

[0051] The preparation process of the geopolymer grouting material provided in this embodiment is as follows:

[0052] (1) Weigh the following components in parts by weight: 300 g fly ash, 200 g cement, 75 g water glass, 3.5 g sodium methyl silicate, and 400 mL water.

[0053] Add fly ash, cement and sodium methyl silicate into a rotary mixer and stir for 3 minutes. After fully mixing, the mixed material is packaged for later use.

[0054] (2) The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as A2.

[0055] Example 2

[0056] The geopolymer grouting material provided in this embodiment includes the following components in parts by weight: 60 parts of fly ash, 40 parts of cement, 15 parts of alkaline activator water glass, 0.4 parts of waterproofing agent sodium methyl silicate, and 80 parts of water.

[0057] The fly ash used in this example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0058] Waterproofing agent: sodium methyl silicate, white solid powder, solid content ≥98%.

[0059] In this embodiment, the water-cement ratio is 0.8, that is, water accounts for 0.8 of the total mass of cement and fly ash;

[0060] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0061] The ash ratio is 0.4%, that is, sodium methyl silicate accounts for 0.4% of the total mass of cement and fly ash.

[0062] The preparation process of the geopolymer grouting material provided in this embodiment is as follows:

[0063] (1) Weigh the following components in parts by weight: 300 g fly ash, 200 g cement, 75 g water glass, 2 g sodium methyl silicate, and 400 mL water.

[0064] Add fly ash, cement and sodium methyl silicate into a rotary mixer and stir for 3 minutes. After fully mixing, the mixed material is packaged for later use.

[0065] The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as A1.

[0066] Example 3

[0067] The geopolymer grouting material provided in this embodiment includes the following components in parts by weight: 60 parts of fly ash, 40 parts of cement, 15 parts of alkaline activator water glass, 1 part of waterproofing agent sodium methyl silicate, and 80 parts of water.

[0068] The fly ash used in this example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0069] Waterproofing agent: sodium methyl silicate, white solid powder, solid content ≥98%.

[0070] In this embodiment, the water-cement ratio is 0.8, that is, water accounts for 0.8 of the total mass of cement and fly ash;

[0071] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0072] The ash ratio is 1%, that is, sodium methyl silicate accounts for 1% of the total mass of cement and fly ash.

[0073] The preparation process of the geopolymer grouting material provided in this embodiment is as follows:

[0074] (1) Weigh the following components in parts by weight: 300 g fly ash, 200 g cement, 75 g water glass, 5 g sodium methyl silicate, and 400 mL water.

[0075] Add fly ash, cement and sodium methyl silicate into a rotary mixer and stir for 3 minutes. After fully mixing, the mixed material is packaged for later use.

[0076] The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as A3.

[0077] Example 4

[0078] The geopolymer grouting material provided in this embodiment includes the following components in parts by weight: 60 parts of fly ash, 40 parts of cement, 15 parts of alkaline activator water glass, 0.4 parts of waterproofing agent isobutyl triethoxy silane, and 80 parts of water.

[0079] The fly ash used in this example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0080] In this embodiment, the water-cement ratio is 0.8, that is, water accounts for 0.8 of the total mass of cement and fly ash;

[0081] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0082] The ash ratio is 0.4%, that is, sodium methyl silicate accounts for 0.4% of the total mass of cement and fly ash.

[0083] The preparation process of the geopolymer grouting material provided in this embodiment is as follows:

[0084] (1) Weigh the following components in parts by weight: 300 g fly ash, 200 g cement, 75 g water glass, 2 g isobutyltriethoxysilane, and 400 mL water.

[0085] Add fly ash, cement and isobutyl triethoxysilane into a rotary mixer and stir for 3 minutes. After fully mixing, the mixed material is packaged for later use.

[0086] (3) The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as A4.

[0087] Example 5

[0088] The geopolymer grouting material provided in this embodiment includes the following components in parts by weight: 60 parts of fly ash, 40 parts of cement, 15 parts of alkaline activator water glass, 0.7 parts of waterproofing agent isobutyl triethoxy silane, and 80 parts of water.

[0089] The fly ash used in this example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0090] In this embodiment, the water-cement ratio is 0.8, that is, water accounts for 0.8 of the total mass of cement and fly ash;

[0091] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0092] The ash ratio is 0.7%, that is, sodium methyl silicate accounts for 0.7% of the total mass of cement and fly ash.

[0093] The preparation process of the geopolymer grouting material provided in this embodiment is as follows:

[0094] (1) Weigh the following components in parts by weight: 300 g fly ash, 200 g cement, 75 g water glass, 3.5 g isobutyltriethoxysilane, and 400 mL water.

[0095] Add fly ash, cement and isobutyl triethoxysilane into a rotary mixer and stir for 3 minutes. After fully mixing, the mixed material is packaged for later use.

[0096] The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as A5.

[0097] Example 6

[0098] The geopolymer grouting material provided in this embodiment includes the following components in parts by weight: 60 parts of fly ash, 40 parts of cement, 15 parts of alkaline activator water glass, 1 part of waterproofing agent isobutyl triethoxy silane, and 80 parts of water.

[0099] The fly ash used in this example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0100] In this embodiment, the water-cement ratio is 0.8, that is, water accounts for 0.8 of the total mass of cement and fly ash;

[0101] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0102] The ash ratio is 1%, that is, sodium methyl silicate accounts for 1% of the total mass of cement and fly ash.

[0103] The preparation process of the geopolymer grouting material provided in this embodiment is as follows:

[0104] (1) Weigh the following components in parts by weight: 300 g fly ash, 200 g cement, 75 g water glass, 5 g isobutyltriethoxysilane, and 400 mL water.

[0105] Add fly ash, cement and isobutyl triethoxysilane into a rotary mixer and stir for 3 minutes. After fully mixing, the mixed material is packaged for later use.

[0106] The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as A6.

[0107] Example 7

[0108] The geopolymer grouting material provided in this embodiment includes the following components in parts by weight: 60 parts of fly ash, 40 parts of cement, 11 parts of alkaline activator water glass, 1 part of waterproofing agent isobutyl triethoxy silane, and 100 parts of water.

[0109] The fly ash used in this example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0110] In this embodiment, the water-cement ratio is 0.8, that is, water accounts for 0.8 of the total mass of cement and fly ash;

[0111] The ash ratio is 1%, that is, sodium methyl silicate accounts for 1% of the total mass of cement and fly ash.

[0112] The preparation process of the geopolymer grouting material provided in this embodiment is as follows:

[0113] (1) Weigh the following components in parts by weight: 600 g fly ash, 400 g cement, 100 g water glass, 10 g isobutyltriethoxysilane, and 1000 mL water.

[0114] Add fly ash, cement and isobutyl triethoxysilane into a rotary mixer and stir for 5 minutes. After fully mixing, the mixed material is packaged for later use.

[0115] The mixed material and water are wet-mixed for 8 minutes to form a slurry, and then water glass is added and quickly stirred for 1 minute to obtain the grouting material.

[0116] Example 8

[0117] The geopolymer grouting material provided in this embodiment includes the following components in parts by weight: 90 parts of fly ash, 10 parts of cement, 20 parts of alkaline activator water glass, 1 part of waterproofing agent isobutyl triethoxy silane, and 90 parts of water.

[0118] The fly ash used in this example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0119] In this embodiment, the water-cement ratio is 0.8, that is, water accounts for 0.8 of the total mass of cement and fly ash;

[0120] The ash ratio is 1%, that is, sodium methyl silicate accounts for 1% of the total mass of cement and fly ash.

[0121] The preparation process of the geopolymer grouting material provided in this embodiment is as follows:

[0122] (1) Weigh the following components in parts by weight: 900 g fly ash, 100 g cement, 200 g water glass, 10 g isobutyltriethoxysilane, and 900 mL water.

[0123] Add fly ash, cement and isobutyl triethoxysilane into a rotary mixer and stir for 4 minutes. After fully mixing, the mixed material is packaged for later use.

[0124] The mixed material and water are wet-mixed for 7 minutes to form a slurry, and then water glass is added and quickly stirred for 1 minute to obtain the grouting material.

[0125] Comparative Example 1

[0126] The geopolymer grouting material provided in this comparative example comprises the following components in parts by weight: 60 parts of fly ash, 40 parts of cement, 15 parts of alkaline activator water glass, and 80 parts of water.

[0127] The fly ash used in this comparative example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0128] In this comparative example, the water-cement ratio is 0.8, i.e., water accounts for 0.8 of the total mass of cement and fly ash;

[0129] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0130] The preparation process of the geopolymer grouting material provided in this comparative example is as follows:

[0131] (1) Weigh the following components in parts by weight: 300 g fly ash, 200 g cement, 75 g water glass, and 400 mL water.

[0132] Add fly ash and cement into a rotary mixer and stir for 3 to 5 minutes. After fully mixing, the mixed material is packaged for later use.

[0133] The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as A0.

[0134] Comparative Example 2

[0135] The geopolymer grouting material provided in this comparative example comprises the following components in parts by weight: 70 parts of fly ash, 30 parts of cement, 15 parts of alkaline activator water glass, and 80 parts of water.

[0136] The fly ash used in this comparative example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0137] In this comparative example, the water-cement ratio is 0.8, i.e., water accounts for 0.8 of the total mass of cement and fly ash;

[0138] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0139] The preparation process of the geopolymer grouting material provided in this comparative example is as follows:

[0140] (1) Weigh the following components according to their weight: 350 g fly ash, 150 g cement, 75 g water glass, and 400 mL water.

[0141] Add fly ash and cement into a rotary mixer and stir for 3 to 5 minutes. After fully mixing, the mixed material is packaged for later use.

[0142] The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as B1.

[0143] Comparative Example 3

[0144] The geopolymer grouting material provided in this comparative example comprises the following components in parts by weight: 80 parts of fly ash, 20 parts of cement, 15 parts of alkaline activator water glass, and 80 parts of water.

[0145] The fly ash used in this comparative example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0146] In this comparative example, the water-cement ratio is 0.8, i.e., water accounts for 0.8 of the total mass of cement and fly ash;

[0147] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0148] The preparation process of the geopolymer grouting material provided in this comparative example is as follows:

[0149] (1) Weigh the following components in parts by weight: 400 g fly ash, 100 g cement, 75 g water glass, and 400 mL water.

[0150] Add fly ash and cement into a rotary mixer and stir for 3 to 5 minutes. After fully mixing, the mixed material is packaged for later use.

[0151] The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as B2.

[0152] Comparative Example 4

[0153] The geopolymer grouting material provided in this comparative example comprises the following components in parts by weight: 90 parts of fly ash, 10 parts of cement, 15 parts of alkaline activator water glass, and 80 parts of water.

[0154] The fly ash used in this comparative example has a fineness of 8.3% (residue on a 45 μm square mesh sieve) and a loss on ignition of 3.1%. The water glass used in this example has a modulus of 3.35 and a density (20° C.) of 1.51 g / mL.

[0155] In this comparative example, the water-cement ratio is 0.8, i.e., water accounts for 0.8 of the total mass of cement and fly ash;

[0156] The slurry ratio is 1:0.2, that is, the volume ratio of cement, fly ash and water to water glass is 1:0.2;

[0157] The preparation process of the geopolymer grouting material provided in this comparative example is as follows:

[0158] (1) Weigh the following components according to their weight: 450 g fly ash, 50 g cement, 75 g water glass, and 400 mL water.

[0159] Add fly ash and cement into a rotary mixer and stir for 3 to 5 minutes. After fully mixing, the mixed material is packaged for later use.

[0160] The mixed material and water were wet-mixed for 5 minutes to form a slurry, and then water glass was added and quickly stirred for 1 minute to obtain a grouting material. The obtained sample was recorded as B3.

[0161] The geopolymer grouting materials prepared in Examples 1-6 and Comparative Examples 1-4 were tested, and the test process and data are as follows:

[0162] 1. Determination of physical properties of materials

[0163] The physical properties of the mixed slurry material are tested in accordance with the "Standard for Test Methods of Ordinary Concrete Mixture Performance" (GB / T 50080-2016) and the "Standard for Test Methods of Physical and Mechanical Properties of Concrete" (GB / T 50081-2019). The test indicators and methods are as follows:

[0164] 1. Fluidity

[0165] Place the sample into a pure slurry fluidity test mold with an upper diameter of 36mm, a lower diameter of 60mm, and a height of 60mm. Scrape it flat with a scraper, lift the test mold in the vertical direction, and start timing at the same time. Allow the geopolymer to flow on the glass plate for 30s, and use a ruler to measure the maximum diameters of the flowing part in three different directions perpendicular to each other. The average value is the fluidity of the sample.

[0166] It can be seen from the test that the fluidity of the geopolymer grouting material prepared in Example 1 is 309 mm.

[0167] 2. Initial setting time and final setting time

[0168] Place the sample into the circular mold of the Vicat instrument and smooth it. First, use the initial setting test needle for measurement. Lower the test needle to contact the sample surface. After tightening the screws, suddenly release it, and the test needle sinks vertically and freely into the sample. Observe the pointer reading when the test needle stops sinking or releases the test needle for 30 seconds. When the test needle sinks to 4±1mm from the bottom plate, the sample reaches the initial setting state. Record the time and subtract it from the time when the material components are added to the mixing bucket. The calculated result is the initial setting time of the sample. After completing the initial setting time measurement, immediately remove the test mold together with the slurry from the glass plate by translation and flip it 180°. Place it on the glass plate with the large end facing up and the small end facing down. Use the final setting test needle for testing. When the test needle can hardly leave a mark on the hardened mixture, record the time and subtract it from the time when the material components are added to the mixing bucket. The calculated result is the final setting time of the sample.

[0169] It can be seen from the test that the initial setting time of the geopolymer grouting material prepared in Example 1 is 8 minutes, and the final setting time is 32 minutes.

[0170] 3. Viscosity

[0171] Take a coating cup and place it on a horizontal surface. Block the outflow hole of the metal funnel and slowly pour the sample into the funnel until the liquid surface protrudes from the edge of the funnel. Scrape off the protruding liquid surface and bubbles along the horizontal surface of the edge. Loosen the outflow hole and start timing at the same time. The test solution flows out in a continuous line. When the outflow line from the orifice is disconnected, stop timing and record the stopwatch reading t. Use formula (1) and formula (2) to calculate the kinematic viscosity γ.

[0172] When t<23s, t=0.154μ+11 (1)

[0173] When 23s≤t≤150s, t=0.223μ+6 (2)

[0174] Where, t represents the outflow time, the unit is s; μ represents the kinematic viscosity, the unit is mm 2 / s.

[0175] It can be seen from the test that the viscosity of the geopolymer grouting material prepared in Example 1 is 13.08 mm 2 / s.

[0176] 4. Compressive strength

[0177] Pour the slurry into a 70.7×70.7×70.7mm triple mold, vibrate it with a vibration table for 120s, scrape off the excess slurry and place it horizontally in a curing box for 24h of curing before demoulding. After demoulding, place it in 20℃±1℃ water for curing. Take out the test block samples that have been cured for the corresponding number of days and wipe the surface dry. Load the compression fixture with a pressure plate area of ​​70.7×70.7mm on the electro-hydraulic servo hydraulic pressure testing machine, take the sample specimen and place it between the upper and lower pressure plates, align the center of the specimen with the center of the pressure plate of the testing machine, and continue to load at a constant rate until the specimen is completely destroyed. The ultimate load is recorded as the compressive strength of the sample. Strength tests at various ages are carried out during curing: the time is 3d±2h, 7d±4h, 14d±6h, and 28d±8h respectively.

[0178] Figure 1 The compressive strength of the geopolymer grouting materials prepared in Examples 1 to 6 and Comparative Examples 1 to 4. Figure 1It can be seen that the compressive strength of all geopolymer grouting materials increases with the increase of curing days. When the fly ash: cement mass ratio is 3:2, the water-solid ratio is 0.8, and the slurry ratio is 1:0.2, the prepared A0 geopolymer grouting material has a compressive strength of 4.26MPa at 28d. In A1, A2 and A3 geopolymer grouting materials, with the gradual increase of the amount of sodium methyl silicate added, the compressive strength of the fly ash-cement-based grouting material first increases and then decreases. Sodium methyl silicate can form an insoluble resin film on the surface of the material through chemical reaction, increase the hydrophobicity of the surface of the grouting material, and can also improve the concrete structure and increase the density, thereby increasing the compressive strength of the material. When 0.4% sodium methyl silicate is added to the ash ratio, the short-term coagulation and hardening effect of the grouting material is slightly enhanced, and the 28d compressive strength increases to 4.88MPa. When 0.7% sodium methyl silicate was added to the ash ratio, the short-term compressive strength of the slurry stone body increased significantly, and its 28d compressive strength reached a maximum of 5.89MPa. However, when excessive sodium methyl silicate was added (accounting for 1% of the ash ratio), the compressive strength of the specimen decreased.

[0179] In A4, A5 and A6 geopolymer grouting materials, after adding 0.4%, 0.7% and 1% isobutyl triethoxysilane by ash mass ratio respectively, the compressive strength of geopolymer grouting materials decreased in the short term. The 28d compressive strength of A4 and A6 test blocks was slightly higher than that of A0 test block, which were 4.57MPa and 4.14MPa respectively. The 28d compressive strength of A6 test block was the lowest, which was 2.9MPa. When isobutyl triethoxysilane is applied on the surface of concrete as a protective coating, the compressive strength can be slightly improved. However, when it is used as an internal admixture, the hydrophobic properties of the concrete itself and the uneven distribution of the hydrophobic film inside the material may affect the cement hydration reaction and coagulation process, causing the compressive strength of the test block to show irregular changes.

[0180] In order to explore the effect of cement ratio in ash on the compressive strength of geopolymer grouting materials, geopolymer grouting materials B1-B3 with cement ratios of 30%, 20%, and 10% were prepared, and the compressive strength was tested after reaching the corresponding curing days. The results showed that after reducing the cement ratio, the compressive strength of the geopolymer grouting materials decreased significantly in the short term of curing. The compressive strength of the geopolymer grouting materials B1-B3 was at a low level at 7d, and the compressive strength of the geopolymer grouting materials B2 and B3 did not reach 1MPa at 28d. The strength of the B1 test block began to increase significantly at 14d, and reached 3.21MPa at 28d. It can be seen that in order to ensure that the geopolymer grouting materials can meet certain physical strength performance requirements, the cement ratio in the slurry preparation must be no less than 30%.

[0181] 3. Determination of heavy metal leaching toxicity of materials

[0182] The slurry was poured into a 70.7mm×70.7mm×70.7mm triple mold, and vibrated for 120s using a vibrating table. After scraping off the excess slurry, it was placed horizontally in a curing box and cured for 24 hours to prepare a test block before demoulding. Because the slurry solidification environment in actual engineering applications is acidic mine water, the heavy metal leaching toxicity test of the raw materials and test blocks was carried out in accordance with the "Solid Waste Leaching Toxicity Leaching Method-Sulfuric Acid and Nitric Acid Method" (HJ / T 299-2007). A mixture of concentrated sulfuric acid and concentrated nitric acid with a mass ratio of 2:1 was added to reagent water to prepare the leaching agent, and the pH value of the solution was 3.20±0.05. The sample was crushed to a particle size of less than 9.5mm, 6-10g of the sample was weighed and placed in an extraction bottle, and the leaching agent was added at a liquid-solid ratio of 10:1 (mL / g). After the bottle cap was tightly closed, it was fixed on a flip-type oscillating device, the speed was adjusted to 30r / min, and oscillated at 23℃ for 18h. Install the filter membrane on the pressure filter, rinse the filter and the filter membrane with dilute nitric acid, discard the elution, filter and collect the leachate. According to the "Hazardous Waste Identification Standard - Leaching Toxicity Identification" (GB 5085.3-2007), the heavy metal concentration in the leachate is measured and identified. The specific detection indicators and methods are shown in Table 3. The heavy metal leaching toxicity test results of the raw materials and the material test blocks are shown in Table 4.

[0183] Table 3 Heavy metal element leaching concentration detection method table

[0184]

[0185] Table 4 Heavy metal leaching toxicity of raw materials and test blocks

[0186]

[0187]

[0188] Note: ND means not detected

[0189] As can be seen from Table 4, the heavy metal leaching concentrations of the four groups of samples are all lower than the allowable limit (GB 5085.3-2007). Only a small amount of Cr element is leached in the raw material cement, a small amount of Cr element and a trace amount of Cd element are leached in the fly ash, and no other heavy metal elements are detected. After the raw materials are prepared into geopolymers, the Cr leaching concentration in the A2 and A4 test blocks is greatly reduced, and no Cd is detected. The fly ash-cement-based geopolymer grouting material prepared in the present invention exhibits a good curing effect on heavy metals due to the large amount of silicate gel products present in it. Among them, since the internal gel products in the A4 geopolymer grouting material are relatively more, the adsorption effect on heavy metals is stronger, and the curing stability is higher, so the Cr leaching concentration is lower. In summary, the geopolymer grouting material provided by the present invention has good physical properties, meets the technical requirements of coal mine stratum grouting construction, and has extremely small heavy metal leaching toxicity, is environmentally friendly, and has no secondary pollution.

[0190] The geopolymer grouting material prepared in Example 1 was used in an indoor dynamic grouting and plugging experiment to treat acid mine water, and its application effect was simulated and tested. The proportion of acid mine water is shown in Table 5.

[0191] Table 5 Water quality ratio of simulated acid mine water

[0192]

[0193] A transparent plexiglass tube with a length of 1m, an inner diameter of 10cm and a wall thickness of 1.5cm was used as a sandstone aquifer simulation container. The container was filled with quartz sand with a particle size of 2 to 4mm. Acidic mine water was continuously introduced into one end of the container with an inlet pressure of 100kPa, and water flowed out naturally from the other end.

[0194] A hole was drilled just above the middle of the container, and the prepared slurry and alkaline activator were injected into the container at a pressure of 150 kPa simultaneously by the double-liquid grouting method. The flow rate at the water outlet of the container was monitored after 8 hours of continuous operation. The converted water blocking rate was 98.18%. The test results of pollutant concentration at the water outlet are shown in Table 6.

[0195] Table 6 Experimental results of simulated dynamic grouting to treat acid mine water

[0196]

[0197]

[0198] In summary, the geopolymer grouting material provided by the present invention has good resistance to hydraulic shock load and acid mine water erosion, and has good water flow blocking effect and water quality improvement effect. This is because the slurry can still provide a certain alkalinity under dynamic water conditions to neutralize the acidity of the solution and increase the pH. At the same time, the erosion of acid mine water promotes the increase of gel products such as C-(A)-SH in the geopolymer, strengthens the ability of the slurry to solidify and stabilize heavy metals, captures and solidifies Fe and Mn ions in the solution and firmly adsorbs them to form Ca4Fe2Cl2(OH) 12 (H2O)4, Mn(OH)2 and Ca4Al2Cl(SO4) 0.5 (OH) 12 (H2O)6 and other new phases are solidified, and SO4 in the solution 2- With the help of H + It erodes the interior of the stone and participates in the deconstruction of the gel and the formation of sulfur-containing minerals such as CaSO4, FeS, and calcium vanadium.

[0199] After 8 hours of continuous operation, X-ray diffraction analysis was performed on the A0, A2, and A4 fly ash-cement-based geopolymer grouting material test blocks after acid mine water curing to observe the phase changes and crystal composition. The specific results are as follows: Figure 2 .from Figure 2 It can be seen from the results that, unlike the results of tap water curing, the most significant crystal diffraction peaks of each test block are transformed from mullite and SiO2 to CaCO3, indicating that under the erosion of the curing solution (AMD), part of SiO2 is decomposed to participate in the formation process of geopolymers, and the silicon-oxygen or aluminum-oxygen tetrahedral structures of some geopolymers are also destroyed by H in AMD. + destroyed. The hydration process of cement is significantly accelerated, resulting in the rapid generation of a large amount of CaCO3, which is one of the reasons why the strength growth period of the material in AMD is greatly shortened and the optimal compressive strength of the specimen is reached ahead of schedule. Among them, the A2 specimen has the relatively highest CaCO3 crystal diffraction peak intensity, indicating that the addition of sodium methyl silicate can further improve the cement hydration degree of the specimen in AMD and provide the material with a certain acid corrosion resistance, while the A4 specimen has the relatively highest mullite crystal diffraction peak intensity, indicating that isobutyltriethoxysilane has a positive effect on the formation process of geopolymers, and its rapidly generated hydrophobic film also provides a certain protection for the cement hydration process. Therefore, it is observed that the CaCO3 crystal peak intensity of the A4 specimen is higher than that of A0. It shows that the addition of sodium methyl silicate can further improve the cement hydration degree of the specimen in AMD and provide the material with a certain acid corrosion resistance. The addition of sodium methyl silicate causes the pH of the curing solution (AMD) to rise slightly, because the silicate generated by hydrolysis reacts with Ca in cement. 2+ The reaction produces calcium silicate hydrate, which promotes the cement hydration reaction.

[0200] When the raw materials in the present invention are purchased, the price of fly ash is 200 yuan / ton, the price of cement is 300 yuan / ton, the price of water glass is 650 yuan / ton, and the price of sodium methyl silicate is 5000 yuan / ton.

[0201] The total cost is as follows: (200*60+300*40+650*15+5000*0.7) / 115.7=353.4 yuan / ton.

[0202] The grouting material commonly used in the prior art is a slurry obtained by mixing cement and water glass, the volume ratio of cement to water glass is 1:0.5, and the cost is 475 yuan / ton. The geopolymer grouting material provided by the present invention greatly reduces the cost of raw materials.

[0203] The geopolymer grouting material prepared by the present invention needs to be used in accordance with the following conditions when used:

[0204] (1) The slurry fluidity of geopolymer grouting material is greater than 270 mm;

[0205] (2) The slurry setting time of geopolymer grouting material is adjusted between 0.3h and 2h;

[0206] (3) The slurry viscosity of geopolymer grouting material is 5mm 2 / s~20mm 2 / s adjustment;

[0207] (4) The compressive strength of the stone body of the geopolymer grouting material is adjusted between 3MPa and 6MPa.

[0208] Although preferred embodiments of the present invention have been described, additional changes and modifications may be made to these embodiments by those skilled in the art once the basic inventive concepts are known. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A geopolymer grouting material, characterized in that: It is composed of serum and alkaline stimulant; The slurry is composed of fly ash, cement, waterproofing agent and water; the mass ratio of fly ash to cement is 6-9:1-4; the amount of waterproofing agent added is 0.4%-0.7% of the total mass of fly ash and cement; the amount of water added is 0.8-1% of the total mass of fly ash and cement; The mass ratio of the alkaline activator to the fly ash is 11-20:60-90.

2. A geopolymer grouting material according to claim 1, characterized in that: The mass ratio of fly ash to cement is 3:

2.

3. A geopolymer grouting material according to claim 1, characterized in that: The amount of waterproofing agent added is 0.7% of the total mass of fly ash and cement.

4. A geopolymer grouting material according to claim 1, characterized in that: The mass ratio of alkaline activator to fly ash is 1:

4.

5. A geopolymer grouting material according to claim 1, characterized in that: The alkaline activator is water glass, the modulus of water glass is 3.11-3.40, and the density is 1-5g / ml.

6. A geopolymer grouting material according to claim 1, characterized in that: The waterproofing agent is sodium methyl silicate or isobutyltriethoxysilane.

7. A geopolymer grouting material according to claim 1, characterized in that: The specific surface area of ​​cement is 0.1m 2 / g~20m 2 / g; The fly ash has a sieve residue of 1% to 30% on a 45μm square hole sieve and a loss on ignition of 1% to 10%.

8. A method for preparing the geopolymer grouting material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Weigh fly ash and cement in a fly ash to cement mass ratio of 6 to 9:1 to 4; weigh the waterproofing agent in an amount of 0.4% to 0.7% of the total mass of fly ash and cement; weigh water in an amount of 0.8% to 1% of the total mass of fly ash and cement; Weigh the alkaline activator according to the mass ratio of alkaline activator to fly ash of 11-20:60-90; Fly ash, cement and waterproofing agent are mixed once to obtain a mixed material; The mixed material is mixed with water for a second time to obtain a mixed slurry; The mixed slurry is mixed with the alkaline activator three times to obtain the geopolymer grouting material.

9. The method for preparing a geopolymer grouting material according to claim 8, characterized in that: The stirring time for the first mixing is 3 minutes to 5 minutes; the stirring time for the second mixing is 5 minutes to 8 minutes.

10. Use of the geopolymer grouting material according to any one of claims 1 to 7 in filling mine surrounding rock cracks or coalfield goaf, characterized in that: The slurry in the geopolymer grouting material and the alkaline activator are injected into the formation by the double-liquid grouting method.

Citation Information

Patent Citations

  • Low heat composite cementing material

    CN102617057A

  • Filling and consolidating powder for mining purposes and use thereof

    CN102887693A

  • Geopolymer composition, geopolymer material and preparation method of geopolymer material

    CN104098281A

  • Rigid self-waterproofing concrete and self-waterproofing building structure

    CN106630860A

  • Geopolymer grouting material and preparation method thereof

    CN117510134A