Monoclinic Ba1-xCaxAl2Si2O8 ceramic material and preparation method thereof
By using high-purity barium carbonate, calcium carbonate, alumina and fused silica, the preparation process of monoclinic barium feldspar ceramic materials is simplified, the problems of high energy consumption and long production cycle are solved, and high purity and low energy consumption are achieved The production of monoclinic Ba1-xCaxAl2Si2O8 ceramic materials is suitable for high-temperature composite materials.
Patent Information
- Application Number
- CN202411184329.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The existing preparation methods of monoclinic barium feldspar ceramic materials have problems such as high energy consumption, long production cycle, complex process and difficult to guarantee purity. Especially at high temperatures, it requires a large amount of energy to consume and it is difficult to completely form a single monoclinic barium feldspar. .
Using barium carbonate, calcium carbonate, alumina and fused silica as the main raw materials, it is molded by a wet ball mill and press-forming machine, and heated at 1300-1500°C for 3 to 5 hours, and is cooled naturally to achieve monoclinic Ba1- of solid phase synthesis method. The preparation of xCaxAl2Si2O8 ceramic material eliminates pretreatment steps, simplifies the process and reduces energy consumption.
The preparation of high-purity monoclinic Ba1-xCaxAl2Si2O8 ceramic material is achieved. It has simple process, short production cycle, low energy consumption, and low thermal expansion coefficient of the material. It is suitable as a matrix for high-temperature composite materials, with good thermal matching and chemical compatibility. sex.
Smart Images

Figure CN119080487A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of monoclinic BaAl2Si2O8 ceramic materials. 1- x Ca x Al2Si2O8 ceramic material and preparation method thereof. Background Art
[0002] Barium feldspar (BaAl2Si2O8) has a high melting point (1760℃), excellent anti-oxidation and reduction properties, low thermal expansion coefficient and low dielectric constant. It is a very promising material with great potential application value in the fields of high-temperature structural materials, reflector matrix materials, high-pressure condensers and radar covers.
[0003] The crystal form of barium feldspar is relatively complex, mainly including monoclinic, hexagonal and orthorhombic crystal forms, among which the monoclinic phase and hexagonal phase are the most common. Hexagonal barium feldspar is a metastable phase below 1590℃, and its thermal expansion coefficient is about 8.0×10 -6 / ℃, the hexagonal phase will undergo a reversible transformation with the tetragonal phase at around 300℃, resulting in a volume change of the material (3-4%), and the material will then produce microcracks. Monoclinic baryte is a stable phase below 1590℃, with a low thermal expansion coefficient of about 2.3×10 -6 / ℃, with good thermal matching and chemical compatibility. Therefore, monoclinic barium feldspar can be used as the matrix of high-temperature composite materials, and monoclinic barium feldspar is preferred in the manufacturing process.
[0004] However, in the common synthesis process, hexagonal barium feldspar has better symmetry, simpler structure and easier nucleation. The first precipitated crystal phase is generally metastable hexagonal barium feldspar. Monoclinic barium feldspar cannot be precipitated directly, but is generated by metastable hexagonal barium feldspar through crystal transformation at high temperature, and this process is extremely slow. It often takes a lot of energy to synthesize high-purity monoclinic barium feldspar, so exploring a synthesis process with lower energy consumption will be of great significance to the development of this field.
[0005] At present, the preparation methods of monoclinic barium feldspar materials are usually: 1) Melting method, using SiO2, Al2O3, and BaCO3 as raw materials, first melt at above 2000℃ to form BaO·Al2O3·BaCO3 glass and cool and grind it into glass powder, and then heat it at above 1100℃ for 10h to obtain monoclinic barium feldspar. However, high temperatures above 2000℃ are obviously not suitable for application in actual situations and require a lot of energy. 2) Sol-gel method, using Ba(OH)2·8H2O·Al(NO3)3·9H2O·TEOS as raw materials, and using sol-gel method to prepare BaO-Al2O3-SiO2 ternary system powder. However, it has a long production cycle, high cost, easy to pollute the environment and difficult to apply to large-scale production. 3) Solid-phase synthesis method, using kaolin and barite as raw materials, sintering at above 1500℃ and keeping warm for 5h to synthesize monoclinic barium feldspar. However, it has not been possible to completely form a single monoclinic barium feldspar, and hexagonal barium feldspar still exists, and a large amount of energy is consumed. 4) Ion exchange method, using nitrate solution Li and Ba, ion exchange and heat treatment of various zeolites to destroy the molecular structure. Finally, after crystallization process, monoclinic barium feldspar powder was obtained. However, the regulation of ion exchange amount is quite difficult and some impurities cannot be removed.
[0006] At present, there are patented technologies for preparing monoclinic barium feldspar ceramic materials, such as the patented technology of "a monoclinic barium feldspar ceramic material based on solid phase synthesis and its preparation method" (CN202210953818.X), which discloses a method for preparing monoclinic barium feldspar ceramic materials, wherein the raw materials are a mixture of a barium source, an aluminum silicon source and a supplementary silicon source, wherein: the barium source is barium carbonate or barium hydroxide, the aluminum silicon source is one of mullite, kyanite, andalusite and sillimanite, and the silicon source is supplemented with fused quartz. The reaction temperature of this technology reaches 1500℃, and the insulation time reaches 6h, which requires a lot of energy consumption; the purity of mullite, kyanite, andalusite and sillimanite in the reactants is low, and it is impossible to guarantee whether the impurities therein will affect the product.
[0007] Literature I (Long-González D, López-Cuevas J, Gutiérrez-Chavarría CA, et al. Synthesis of monoclinic Celsian from Coal Fly Ash by using a one-step solid-state reaction process. Ceramics international, 2010, 36 (2): 661-672.) uses fly ash and BaCO3 as the main raw materials, adds Al2O3 and SrCO3 and synthesizes monoclinic celsium feldspar by solid phase synthesis. Since the fly ash raw material has low purity, the Al2O3 and SiO2 components contained are less than 86%, and it contains a lot of other oxide impurities, which will cause uncertain effects on the synthesized monoclinic celsium feldspar. In addition, since the fly ash raw material has low purity, impurities such as Fe2O3 need to be removed by means such as magnetic separation, which has a complex process and a long production cycle, and will consume more energy and time.
[0008] Reference II (Xiaojing Y, Yao Z, Shihua D, et al. Structure and dielectric properties of Ca doped BaAl2Si2O8. Ceramics International, 2018, 44: S43-S45.) uses BaCO3, CaCO3, Al2O3 and SiO2 as raw materials, ball mills for 8 hours and then dries, pre-sinters at 920℃ for 2.5 hours, uniaxially presses at 300MPa, and sinters at 1425℃ for 5 hours to synthesize monoclinic barium feldspar. The two-step method uses pre-sintering, which consumes a lot of time and energy, has a complex process and a long production cycle; and needs to be kept at a high temperature of 1425℃ for 5 hours, which will also consume a lot of energy. Summary of the invention
[0009] The present invention aims to overcome the defects of the prior art and to provide a monoclinic Ba 1-x Ca x Preparation method of Al2Si2O8 ceramic material, prepared monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material has high purity.
[0010] To achieve the above object, the specific steps of the technical solution adopted by the present invention are:
[0011] Step 1, using 35.4-43.3wt% of barium carbonate, 2.5-7.7wt% of calcium carbonate, 24.9-26.1wt% of aluminum oxide and 29.3-30.8wt% of fused quartz as raw materials, mixing them uniformly to obtain a mixture I; then wet-ball milling, drying and crushing the mixture I; then adding 0.04-0.06wt% of sodium carboxymethyl cellulose and 3-5wt% of water to the raw materials, mixing, and obtaining a mixture II.
[0012] Step 2: Press the mixed material II into a shape under the condition of 60-80 MPa, and dry it to obtain a celsium feldspar body.
[0013] Step 3: In an air atmosphere and normal pressure, the celsium feldspar body is heated to 1300-1500°C, kept at this temperature for 3-5 hours, and cooled naturally to obtain monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material.
[0014] The purity of the barium carbonate is greater than 99.0%; the particle size of the barium carbonate is less than 2 μm.
[0015] The purity of the calcium carbonate is greater than 99.0%; the particle size of the calcium carbonate is less than 2 μm.
[0016] The purity of the aluminum oxide is greater than 99.0%; the particle size of the aluminum oxide is less than 75 μm.
[0017] The purity of the fused quartz is greater than 99.5%; the particle size of the fused quartz is less than 75 μm.
[0018] The mass ratio of the grinding balls: the mixed material: the water in the wet ball mill is 2:1:1, and the material of the grinding balls is zirconium oxide.
[0019] The viscosity of the sodium carboxymethyl cellulose is 600-3000 mpa.s.
[0020] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:
[0021] 1. The present invention uses barium carbonate, calcium carbonate, aluminum oxide and fused quartz as main raw materials, and the purity of the raw materials used is greater than 99.0%, which is conducive to the synthesis of high-purity monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material.
[0022] 2. The present invention uses barium carbonate, calcium carbonate, aluminum oxide and fused quartz as raw materials, mixes them according to a formula, ball mills them, and dries them; then presses them into shape, dries them; heats them to 1300-1500°C, keeps them warm for 3 hours, and cools them naturally to prepare monoclinic Ba based on a solid phase synthesis method. 1-x Ca xAl2Si2O8 ceramic material does not require pretreatment of raw materials, and has a simple process and low energy consumption.
[0023] 3. The present invention is to prepare monoclinic Ba from raw material mixing 1-x Ca x Al2Si2O8 ceramic material only takes 1 to 2 days and does not need to be pre-fired. However, the existing solid phase synthesis method has a production cycle of more than 3 days, so the production cycle of the present invention is short.
[0024] 4. The present invention can synthesize high-purity monoclinic Ba by heating to 1300-1500°C and keeping the temperature for 3 hours. 1- x Ca x Al2Si2O8 ceramic material, while the general solid phase synthesis method needs to be heated to 1500°C and kept warm for 5-6 hours, so the present invention has a short cycle and low energy consumption.
[0025] 5. The calcium carbonate used in the present invention can be decomposed into CaO as a mineralizer to form Ba 1-x Ca x Al2Si2O8 interstitial solid solution promotes the nucleation process of the monoclinic phase and the transformation of the hexagonal phase to the monoclinic phase. 1-x Ca x Al2Si2O8 ceramics have high purity. 1-x Ca x As the amount of calcium carbonate added (x) increases, monoclinic BaAl2Si2O8 ceramic materials can be prepared at lower temperatures. 1-x Ca x Al2Si2O8 ceramic material, low energy consumption.
[0026] 6. The calcium carbonate used in the present invention can also be decomposed into CaO as a flux to form a low eutectic with other reactants, thereby reducing the activation energy of the reaction and increasing the reaction rate, thereby promoting the formation of monoclinic basite. 1- x Ca x The main crystal phase of Al2Si2O8 ceramic materials is monoclinic, and the diffraction peak intensity of the hexagonal phase is very low or non-existent. Hexagonal barium feldspar will produce microcracks during actual use, resulting in material cracking and affecting the use of the material. 1-x Ca x Al2Si2O8 ceramic material has high purity, while monoclinic basilite has low thermal expansion coefficient, and has good thermal matching and chemical compatibility. 1-x Ca x Al2Si2O8 ceramic materials can be used as the matrix of high-temperature composite materials and have a wide range of applications.
[0027] The monoclinic Ba prepared by the present invention 1-x Ca x X-ray diffraction analysis of Al2Si2O8 ceramic material shows that the main crystal phase is monoclinic barium feldspar. The purity is 95-98%.
[0028] Therefore, the present invention has the characteristics of simple process, short production cycle and low energy consumption. 1- x Ca x Al2Si2O8 ceramic material has high purity. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Four monoclinic Ba prepared in the present invention 1-x Ca x X-ray diffraction pattern of Al2Si2O8 ceramic material. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods, which does not limit the protection scope of the present invention.
[0031] A monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material and preparation method thereof. The preparation method described in this specific embodiment is:
[0032] Step 1, using 35.4-43.3wt% of barium carbonate, 2.5-7.7wt% of calcium carbonate, 24.9-26.1wt% of aluminum oxide and 29.3-30.8wt% of fused quartz as raw materials, mixing them uniformly to obtain a mixture I; then wet-ball milling, drying and crushing the mixture I; then adding 0.04-0.06wt% of sodium carboxymethyl cellulose and 3-5wt% of water to the raw materials, mixing, and obtaining a mixture II.
[0033] Step 2: Press the mixed material II into a shape under the condition of 60-80 MPa, and dry it to obtain a celsium feldspar body.
[0034] Step 3: In an air atmosphere and normal pressure, the celsium feldspar body is heated to 1300-1500°C, kept at this temperature for 3-5 hours, and cooled naturally to obtain monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material.
[0035] The purity of the barium carbonate is greater than 99.0%;
[0036] The purity of the calcium carbonate is greater than 99.0%;
[0037] The purity of the aluminum oxide is greater than 99.0%;
[0038] The purity of the fused quartz is greater than 99.5%;
[0039] The viscosity of the sodium carboxymethyl cellulose is 600-3000 mpa.s.
[0040] In this specific implementation mode:
[0041] The particle size of the barium carbonate is less than 2 μm;
[0042] The particle size of the calcium carbonate is less than 2 μm;
[0043] The particle size of the aluminum oxide is less than 75 μm;
[0044] The particle size of the fused quartz is less than 75 μm;
[0045] The mass ratio of the grinding balls: the mixed material: the water in the wet ball mill is 2:1:1, and the material of the grinding balls is zirconium oxide.
[0046] This will not be described in detail in the embodiments.
[0047] Example 1
[0048] A monoclinic Ba 0.7 Ca 0.3 Al2Si2O8 ceramic material and preparation method thereof. The preparation method described in this embodiment is:
[0049] Step 1, using 35.4wt% of barium carbonate, 7.7wt% of calcium carbonate, 26.1wt% of aluminum oxide and 30.8wt% of fused quartz as raw materials, mixing them evenly to obtain a mixture I; then wet ball milling, drying and crushing the mixture I; then adding 0.04wt% of sodium carboxymethyl cellulose and 3wt% of water to the raw materials, mixing, and obtaining a mixture II.
[0050] Step 2: Press the mixed material II into a mold under 60 MPa, and dry it to obtain a celsium feldspar body.
[0051] Step 3: In an air atmosphere and normal pressure, the celsium feldspar body is heated to 1300°C, kept at this temperature for 5 hours, and cooled naturally to obtain monoclinic Ba 0.7 Ca 0.3 Al2Si2O8 ceramic material.
[0052] The purity of the barium carbonate is 99.1%;
[0053] The purity of the calcium carbonate is 99.2%;
[0054] The purity of the aluminum oxide is 99.1%;
[0055] The purity of the fused quartz is 99.6%;
[0056] The viscosity of the sodium carboxymethyl cellulose is 600 mPa.s.
[0057] The monoclinic Ba prepared by the present invention 0.7 Ca 0.3 X-ray diffraction analysis of Al2Si2O8 ceramic material shows that the main crystal phase is monoclinic barium feldspar. After testing, the purity is 95.00%.
[0058] Example 2
[0059] A monoclinic Ba 0.8 Ca 0.2 Al2Si2O8 ceramic material and preparation method thereof. The preparation method described in this embodiment is:
[0060] Step 1, 39.5wt% of barium carbonate, 5.0wt% of calcium carbonate, 25.5wt% of aluminum oxide and 30.0wt% of fused quartz are used as raw materials, mixed evenly to obtain a mixture I; the mixture I is then wet-ball milled, dried, and crushed; and then 0.05wt% of sodium carboxymethyl cellulose and 4wt% of water are added to the raw materials, mixed, and a mixture II is obtained.
[0061] Step 2: Press the mixed material II into a mold under 65 MPa and dry it to obtain a celsium feldspar body.
[0062] Step 3: In an air atmosphere and normal pressure, the celsium feldspar body is heated to 1400°C, kept at this temperature for 4.5 hours, and cooled naturally to obtain monoclinic Ba 0.8 Ca 0.2 Al2Si2O8 ceramic material.
[0063] The purity of the barium carbonate is 99.3%;
[0064] The purity of the calcium carbonate is 99.3%;
[0065] The purity of the aluminum oxide is 99.2%;
[0066] The purity of the fused quartz is 99.7%;
[0067] The viscosity of the sodium carboxymethyl cellulose is 1000 mPa.s.
[0068] The monoclinic Ba prepared by the present invention 0.8 Ca 0.2 X-ray diffraction analysis of Al2Si2O8 ceramic material shows that the main crystal phase is monoclinic baryte. After testing, the purity is 97.33%.
[0069] Example 3
[0070] A monoclinic Ba 0.85 Ca 0.15 Al2Si2O8 ceramic material and preparation method thereof. The preparation method described in this embodiment is:
[0071] Step 1, using 41.4wt% of barium carbonate, 3.7wt% of calcium carbonate, 25.2wt% of aluminum oxide and 29.7wt% of fused quartz as raw materials, mixing them evenly to obtain a mixture I; then wet ball milling, drying and crushing the mixture I; then adding 0.06wt% of sodium carboxymethyl cellulose and 5wt% of water to the raw materials, mixing, and obtaining a mixture II.
[0072] Step 2: Press the mixed material II into a mold under 70 MPa and dry it to obtain a celsium feldspar body.
[0073] Step 3: In an air atmosphere and normal pressure, the celsium feldspar body is heated to 1450°C, kept at this temperature for 4 hours, and cooled naturally to obtain monoclinic Ba 0.85 Ca 0.15 Al2Si2O8 ceramic material.
[0074] The purity of the barium carbonate is 99.4%;
[0075] The purity of the calcium carbonate is 99.5%;
[0076] The purity of the aluminum oxide is 99.4%;
[0077] The purity of the fused quartz is 99.7%;
[0078] The viscosity of the sodium carboxymethyl cellulose is 2000 mPa.s.
[0079] The monoclinic Ba prepared by the present invention 0.85 Ca 0.15 X-ray diffraction analysis of Al2Si2O8 ceramic material shows that the main crystal phase is monoclinic baryte. After testing, the purity is 98.00%.
[0080] Example 4
[0081] A monoclinic Ba 0.9 Ca 0.1 Al2Si2O8 ceramic material and preparation method thereof. The preparation method described in this embodiment is:
[0082] Step 1, using 43.3wt% of barium carbonate, 2.5wt% of calcium carbonate, 24.9wt% of aluminum oxide and 29.3wt% of fused quartz as raw materials, mixing them evenly to obtain a mixture I; then wet ball milling, drying and crushing the mixture I; then adding 0.06wt% of sodium carboxymethyl cellulose and 5wt% of water to the raw materials, mixing, and obtaining a mixture II.
[0083] Step 2: Press the mixed material II into a mold under 80 MPa, and dry it to obtain a celsium feldspar body.
[0084] Step 3: In an air atmosphere and normal pressure, the celsium feldspar body is heated to 1500°C, kept at this temperature for 3 hours, and cooled naturally to obtain monoclinic Ba 0.9 Ca 0.1 Al2Si2O8 ceramic material.
[0085] The purity of the barium carbonate is 99.3%;
[0086] The purity of the calcium carbonate is 99.2%;
[0087] The purity of the aluminum oxide is 99.1%;
[0088] The purity of the fused quartz is 99.8%;
[0089] The viscosity of the sodium carboxymethyl cellulose is 3000 mPa.s.
[0090] The monoclinic Ba prepared by the present invention 0.9 Ca 0.1 X-ray diffraction analysis of Al2Si2O8 ceramic material shows that the main crystal phase is monoclinic barium feldspar. The purity is 97.57%.
[0091] Compared with the prior art, this specific implementation has the following positive effects:
[0092] 1. This specific embodiment uses barium carbonate, calcium carbonate, aluminum oxide and fused quartz as main raw materials, and the purity of the raw materials used is greater than 99.0%, which is conducive to the synthesis of high-purity monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material.
[0093] 2. This specific embodiment uses barium carbonate, calcium carbonate, aluminum oxide and fused quartz as raw materials, mixes them according to the formula, ball mills, and dries them; then presses them into shape, dries them; heats them to 1300-1500°C, keeps them warm for 3 hours, and cools them naturally. The monoclinic Ba prepared by the solid phase synthesis method 1-x Ca x Al2Si2O8 ceramic material does not require pretreatment of raw materials, and has a simple process and low energy consumption.
[0094] 3. This specific implementation method is from raw material mixing to preparing monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material only takes 1 to 2 days and does not require pre-firing. However, the existing solid phase synthesis method has a production cycle of more than 3 days, so the production cycle of this specific implementation method is short.
[0095] 4. This specific embodiment only needs to be heated to 1300-1500°C and kept warm for 3 hours to synthesize high-purity monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material, while the general solid phase synthesis method needs to be heated to 1500°C and kept warm for 5-6 hours, so the specific implementation method has a short cycle and low energy consumption.
[0096] 5. The calcium carbonate used in this embodiment can be decomposed into CaO as a mineralizer to form Ba 1- x Ca x Al2Si2O8 interstitial solid solution promotes the nucleation process of the monoclinic phase and the transformation of the hexagonal phase to the monoclinic phase. 1-x Ca x Al2Si2O8 ceramics have high purity. 1-x Ca x Al2Si2O8 ceramic materials such as Figure 1 As shown, Figure 1 The monoclinic Ba prepared in Examples 1 to 4 1-x Ca x X-ray diffraction pattern of Al2Si2O8 ceramic material; Figure 1 It can be seen that with the increase of calcium carbonate addition (x), monoclinic Ba can be prepared at a lower temperature. 1-x Ca x Al2Si2O8 ceramic material, low energy consumption.
[0097] 6. The calcium carbonate used in this embodiment can also be decomposed into CaO as a flux to form a eutectic with other reactants, thereby reducing the activation energy of the reaction and increasing the reaction rate, thereby promoting the formation of monoclinic celsium feldspar. Figure 1 It can be seen that the monoclinic Ba prepared in Examples 1 to 4 1-x Ca x The main crystalline phase of Al2Si2O8 ceramic materials is monoclinic, and the diffraction peak intensity of the hexagonal phase is very low or non-existent. Hexagonal barium feldspar will produce microcracks during actual use, resulting in material cracking and affecting the use of the material. 1-x Ca xAl2Si2O8 ceramic material has high purity, while monoclinic basilite has low thermal expansion coefficient, and has good thermal matching and chemical compatibility. 1-x Ca x Al2Si2O8 ceramic materials can be used as the matrix of high-temperature composite materials and have a wide range of applications.
[0098] The monoclinic Ba prepared in this specific embodiment 1-x Ca x X-ray diffraction analysis of Al2Si2O8 ceramic material shows that the main crystal phase is monoclinic barium feldspar. The purity is 95-98%.
[0099] Therefore, the present embodiment has the characteristics of simple process, short production cycle and low energy consumption. 1-x Ca x Al2Si2O8 ceramic material has high purity.
Claims
1. A monoclinic Ba 1-x Ca x The preparation method of Al2Si2O8 ceramic material is characterized in that The steps of the preparation method are: Step 1, using 35.4-43.3wt% of barium carbonate, 2.5-7.7wt% of calcium carbonate, 24.9-26.1wt% of aluminum oxide and 29.3-30.8wt% of fused quartz as raw materials, mixing them uniformly to obtain a mixture I; then wet-ball milling, drying and crushing the mixture I; then adding 0.04-0.06wt% of sodium carboxymethyl cellulose and 3-5wt% of water to the raw materials, mixing, and obtaining a mixture II; Step 2, pressing the mixed material II under 60-80 MPa, and drying to obtain a celsium feldspar body; Step 3: In an air atmosphere and normal pressure, the celsium feldspar body is heated to 1300-1500°C, kept at this temperature for 3-5 hours, and cooled naturally to obtain monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material.
2. The monoclinic Ba according to claim 1 1-x Ca x The preparation method of Al2Si2O8 ceramic material is characterized in that The purity of the barium carbonate is greater than 99.0%; the particle size of the barium carbonate is less than 2 μm.
3. The monoclinic Ba according to claim 1 1-x Ca x The preparation method of Al2Si2O8 ceramic material is characterized in that The purity of the calcium carbonate is greater than 99.0%; the particle size of the calcium carbonate is less than 2 μm.
4. The monoclinic Ba according to claim 1 1-x Ca x The preparation method of Al2Si2O8 ceramic material is characterized in that The purity of the aluminum oxide is greater than 99.0%; the particle size of the aluminum oxide is less than 75 μm.
5. The monoclinic Ba according to claim 1 1-x Ca x The preparation method of Al2Si2O8 ceramic material is characterized in that The purity of the fused quartz is greater than 99.5%; the particle size of the fused quartz is less than 75 μm.
6. The monoclinic Ba according to claim 1 1-x Ca x The preparation method of Al2Si2O8 ceramic material is characterized in that The mass ratio of the grinding balls: the mixed material: the water in the wet ball mill is 2:1:1, and the material of the grinding balls is zirconium oxide.
7. The monoclinic Ba according to claim 1 1-x Ca x The preparation method of Al2Si2O8 ceramic material is characterized in that The viscosity of the sodium carboxymethyl cellulose is 600-3000 mpa.s.
8. A monoclinic Ba 1-x Ca x Al2Si2O8 ceramic material, characterized by The monoclinic Ba 1-x Ca x The Al2Si2O8 ceramic material is the monoclinic Ba 1-x Ca x Monoclinic Ba prepared by the preparation method of Al2Si2O8 ceramic material 1-x Ca x Al2Si2O8 ceramic material.
Citation Information
Patent Citations
Monoclinic barium feldspar ceramic with low thermal expansion coefficient and preparation method
CN110483029A
Monoclinic phase-based low-dielectric microwave dielectric ceramic material and preparation method thereof
CN111635222A
Super-hydrophobic matrix material of monoclinic-phase celsian glass ceramic and preparation method thereof
CN113735449A
Monoclinic celsian ceramic material based on solid-phase synthesis method and preparation method of monoclinic celsian ceramic material
CN115286374A
Low-loss temperature-stable celsian-based microwave dielectric ceramic material and preparation method thereof