Preparation method of viscose-based short fiber thermal insulation composite material

By preparing viscose-based short fiber insulation composite material, using boron carbide protective layer and porous structure, the problems of insufficient mechanical strength and high thermal conductivity of carbon fiber at high temperatures are solved, and the combination of low thermal conductivity and high mechanical properties is achieved. Excellent insulation for high-temperature equipment.

CN119080520AActive Publication Date: 2024-12-06HENAN GUANHE NEW MATERIAL TECH CO LTD
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
CN202411093313.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-06
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing carbon fiber insulation materials are not mechanically strong at high temperatures and have high thermal conductivity, making it difficult to meet the excellent insulation performance requirements of high-temperature equipment.

Method used

Viscose-based short fibers are used as raw materials, and through pretreatment, chopping, crosslinking and curing and high-temperature cracking reactions, a viscose-based short fiber insulation composite material with low thermal conductivity and high mechanical properties is prepared, using boric acid, polyvinyl alcohol, Excipients such as 2,2-dihydroxybiphenyl, zirconium sol, phenolic resin and polyethyleneimine form a stable boron carbide protective layer and porous structure, improving the dispersion performance and density of the fibers.

Benefits of technology

It achieves low thermal conductivity and excellent mechanical properties, improves the compressive strength and thermal insulation properties of the material, and is suitable for high-temperature equipment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The preparation method comprises the following steps: taking viscose-based carbon fibers as raw materials, chopping the viscose-based carbon fibers, mixing the chopped viscose-based carbon fibers with an auxiliary material A solution, heating the mixed chopped fibers in a vacuum tube furnace to obtain pretreated carbon fibers, mixing an auxiliary material B solution with the pretreated carbon fibers to obtain mixed carbon fibers, putting the mixed carbon fibers into a drying oven, and carrying out cross-linking curing to obtain mixed gel; finally, the mixed gel is subjected to a high-temperature cracking reaction, and the short fiber hard heat preservation composite material is finally prepared and is low in heat conductivity, good in mechanical performance and excellent in density and high-temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermal insulation materials, in particular to a viscose-based short-fiber thermal insulation composite material. Background Art

[0002] Carbon fiber is a new type of fiber material with high strength and high modulus fiber with a carbon content of more than 95%. It is a microcrystalline graphite material obtained by stacking organic fibers such as flake graphite microcrystals along the axial direction of the fiber and undergoing carbonization and graphitization treatment. Carbon fiber thermal insulation materials (such as carbon fiber thermal insulation felt) have excellent properties such as low thermal conductivity, low heat capacity, small linear expansion coefficient, constant mechanical strength at high temperature, corrosion resistance, and light weight. They are widely used in high-temperature vacuum furnaces or inert atmosphere furnaces due to their superior high-temperature resistance, high-temperature thermal insulation performance, easy molding and processing performance, and low impurity content. At present, carbon fiber thermal insulation materials are divided into three categories according to the type of raw materials: polyacrylonitrile (PAN)-based carbon fiber thermal insulation materials, viscose-based carbon fiber thermal insulation materials, and asphalt-based carbon fiber thermal insulation materials. The quality of thermal insulation performance directly affects the operating process and energy consumption of high-temperature equipment. Some studies have reported that viscose-based thermal insulation performance is the best. The present invention provides a method for preparing viscose-based short fibers with excellent thermal insulation performance. Summary of the invention

[0003] The present invention uses viscose-based carbon fiber as a raw material, chops it and mixes it with an auxiliary material A solution, then puts the mixed chopped fibers into a vacuum tube furnace for heating to obtain pretreated carbon fibers, then mixes the auxiliary material B solution with the pretreated carbon fibers to obtain mixed carbon fibers, and puts the mixed carbon fibers into an oven for cross-linking and curing to obtain a mixed gel, and finally performs a high-temperature pyrolysis reaction on the mixed gel to finally obtain a short-fiber hard thermal insulation composite material. The viscose-based short-fiber thermal insulation composite material of the present invention has low thermal conductivity, good mechanical properties, and excellent density and high-temperature resistance.

[0004] A method for preparing a viscose-based short fiber thermal insulation composite material, the method comprising:

[0005] 1) pretreating the viscose fiber, then placing the treated viscose fiber in a tubular furnace, evacuating, heating, introducing water vapor, and keeping the temperature; replacing the introduced water vapor with introducing ammonia, heating, and keeping the temperature; replacing the introduced ammonia with introducing carbon dioxide, keeping the temperature, and then cooling to room temperature to obtain a viscose-based carbon fiber;

[0006] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent, adding ammonia water to adjust the pH value, and obtaining an auxiliary material A solution;

[0007] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution, heating and filtering to obtain a solid;

[0008] 4) placing the product of step 3 into a vacuum tube furnace and heat treating it under nitrogen protection to obtain pretreated carbon fiber;

[0009] 5) dispersing soluble zirconium salt, oxalic acid, polyvinyl alcohol and glycerol in deionized water, stirring evenly to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol to obtain a phenolic resin mixed solution; mixing the zirconium sol and the phenolic resin mixed solution to obtain an auxiliary material B solution;

[0010] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate and dimethyldiethoxysilane are mixed evenly, placed in an oven for heating, and cross-linked and cured to obtain a mixed gel;

[0011] 7) placing the mixed gel in a high-temperature furnace, protecting it with nitrogen, and subjecting it to heat treatment to obtain a viscose-based short fiber thermal insulation composite material.

[0012] Furthermore, the pretreatment process in step 1 includes soaking the viscose fiber in 90-100° C. water for 0.5-3 h, drying, and then soaking in 50-70° C. 3-6wt% diammonium hydrogen phosphate aqueous solution for 0.5-3 h, and drying.

[0013] Furthermore, in the step 1, the treated viscose fiber is placed in a tubular furnace, evacuated, heated to 600-700°C, and water vapor is introduced at a flow rate of 50-100ml / min for 1-2h; the introduced water vapor is replaced by ammonia, the temperature is raised to 850-900°C, the flow rate of ammonia is 50-100ml / min, and the temperature is maintained for 2-4h; the introduced ammonia is replaced by carbon dioxide at a flow rate of 50-100ml / min for 0.2-0.5h, and then the carbon dioxide is kept introduced and cooled to room temperature to obtain viscose-based carbon fiber.

[0014] Furthermore, in step 2, boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl are dispersed in an ethanol solvent in a mass ratio of 1:2-2.5:2-2.5, wherein the mass ratio of boric acid to ethanol is 1:100-150, and ammonia water is added to adjust the pH value to 4-6 to obtain an auxiliary material A solution.

[0015] Furthermore, in the step 3, the short fibers are mixed with the auxiliary material A solution in a mass ratio of 1:1.5-3, heated at 70-90° C. for 3-6 hours, and filtered to obtain a solid.

[0016] Furthermore, in step 4, the product of step 3 is placed in a vacuum tube furnace, heated at 100-150° C. for 1-2 hours under nitrogen protection, and then heated to 1000-1200° C. and heat treated for 4-6 hours to obtain pretreated carbon fiber.

[0017] Furthermore, in the step 5, zirconium nitrate, oxalic acid, polyvinyl alcohol and propylene glycol are dispersed in deionized water in a mass ratio of 100:10-15:5-10:5-10, wherein the mass ratio of zirconium nitrate to deionized water is 10-15:100; the mixture is stirred at 80-90°C to obtain a zirconium sol; phenolic resin and polyethyleneimine are dispersed in ethanol in a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 3-6:100; the zirconium sol and the phenolic resin mixed solution are mixed in a mass ratio of 1:1.5-2 to obtain an auxiliary material B solution.

[0018] Furthermore, in step 6, the pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are evenly mixed in a mass ratio of 100:100-120:5-10:5-10, and then placed in an oven for heating for 2-6 hours to cross-link and cure to obtain a mixed gel.

[0019] Furthermore, in step 7, the mixed gel is placed in a high-temperature furnace, protected by nitrogen, heated at 800-900° C. for 5-7 hours, and then heated to 2000-2200° C. for 0.5-1 hour to obtain a viscose-based short fiber thermal insulation composite material.

[0020] Furthermore, a viscose-based short fiber thermal insulation composite material is provided, characterized in that the material is prepared by the method described.

[0021] Beneficial technical effects of the present invention

[0022] The beneficial effects of the present invention compared with the traditional process are:

[0023] 1) By oxidizing the viscose fiber at high temperature under water vapor, oxidized groups are generated on the surface of the viscose fiber, thereby improving the activation efficiency of the amino groups on its surface by ammonia at high temperature. Then the nitrogen-containing groups react with the subsequently added carbon dioxide at high temperature, thereby generating groups containing carbonized nitrogen on the fiber surface. The carbonized nitrogen groups can improve the surface activity of the fiber and at the same time, can also improve the mechanical strength of the fiber;

[0024] 2) Boric acid and polyvinyl alcohol can form a stable high-temperature protective layer of boron carbide on the surface of pretreated carbon fiber under the action of 2,2-dihydroxybiphenyl at high temperature, thereby reducing the degradation rate of carbon fiber during subsequent high-temperature carbonization, protecting carbon fiber and providing excellent mechanical properties. In addition, the presence of boron carbide can also effectively improve the interface bonding state between fiber and zirconium dioxide ceramic.

[0025] 3) By mixing zirconium sol, phenolic resin and polyethyleneimine, the carbon fiber can be dispersed more evenly during the dispersion process due to the charge adsorption capacity of polyethyleneimine, thereby improving the dispersion performance of the carbon fiber in the gel and the mechanical properties of the material. In addition, the chopped carbon fiber and ceramic powder can increase the packing density of the gel. At the same time, the phenolic resin and polyethyleneimine are cracked into porous carbon during the high-temperature carbonization process, thereby improving the density and strength of the thermal insulation material while improving the thermal insulation performance. DETAILED DESCRIPTION

[0026] The present invention will be described in more detail below through specific embodiments, but the protection scope of the present invention is not limited to these embodiments.

[0027] Embodiment 1:

[0028] 1) soaking the viscose fiber in 90°C water for 3h, drying, and then soaking in a 3wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60°C for 3h, drying, placing the dried product in a tubular furnace, evacuating, heating to 600°C, introducing water vapor at a flow rate of 50ml / min, and maintaining for 1h; replacing the introduced water vapor with ammonia, heating to 850°C, with a flow rate of 50ml / min, and maintaining for 2h; replacing the introduced ammonia with carbon dioxide at a flow rate of 50ml / min, and maintaining for 0.5h, and then cooling to room temperature while maintaining the carbon dioxide to obtain a viscose-based carbon fiber;

[0029] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent in a mass ratio of 1:2:2, wherein the mass ratio of boric acid to ethanol is 1:100, and adding ammonia water to adjust the pH value to 4 to obtain an auxiliary material A solution;

[0030] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing the short fibers with the auxiliary material A solution at a mass ratio of 1:1.5, heating at 70° C. for 3 h, and filtering to obtain a solid;

[0031] 4) placing the product of step 3 into a vacuum tube furnace, heating at 100° C. for 1 h under nitrogen protection, then heating to 1000° C. and heat treating for 4 h to obtain pretreated carbon fiber;

[0032] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:10:5:5, wherein the mass ratio of zirconium nitrate to deionized water is 10:100; stirring evenly at 80° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 3:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.5 to obtain an auxiliary material B solution;

[0033] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:100:5:5, and then placed in an oven for heating for 2 hours to cross-link and solidify to obtain a mixed gel;

[0034] 7) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 900° C. for 5 h, and then heated to 2000° C. for 1 h to obtain a viscose-based short fiber thermal insulation composite material.

[0035] Embodiment 2:

[0036] 1) Soak the viscose fiber in 100° C. water for 1 hour, dry it, and then soak it in a 4wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60° C. for 1 hour, dry it, place the dried product in a tube furnace, evacuate it, heat it to 700° C., introduce water vapor at a flow rate of 100 ml / min, and keep it for 2 hours; replace the introduced water vapor with ammonia, heat it to 900° C., and the flow rate of ammonia is 100 ml / min, and keep it for 4 hours; replace the introduced ammonia with carbon dioxide at a flow rate of 100 ml / min, and keep it for 0.5 hours, and then keep the carbon dioxide introduced and cool it to room temperature to obtain a viscose-based carbon fiber;

[0037] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent in a mass ratio of 1:2.5:2.5, wherein the mass ratio of boric acid to ethanol is 1:150, adding ammonia water to adjust the pH value to 5, to obtain an auxiliary material A solution;

[0038] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution at a mass ratio of 1:3, heating at 90° C. for 3 h, and filtering to obtain a solid;

[0039] 4) placing the product of step 3 into a vacuum tube furnace, heating at 100° C. for 2 h under nitrogen protection, then heating to 1200° C. and heat treating for 4 h to obtain pretreated carbon fiber;

[0040] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:12:7:7, wherein the mass ratio of zirconium nitrate to deionized water is 12:100; stirring evenly at 90° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 4:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:2 to obtain an auxiliary material B solution;

[0041] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:110:6:6, and then placed in an oven for heating for 4 hours to cross-link and cure to obtain a mixed gel;

[0042] 7) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 800° C. for 7 h, and then heated to 2000° C. for 1 h to obtain a viscose-based short fiber thermal insulation composite material.

[0043] Embodiment 3:

[0044] 1) soaking the viscose fiber in 90°C water for 3 hours, drying, and then soaking it in a 6wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60°C for 3 hours, drying, placing the dried product in a tubular furnace, evacuating, heating to 650°C, introducing water vapor at a flow rate of 80 ml / min, and maintaining for 1 hour; replacing the introduced water vapor with ammonia, heating to 900°C, with a flow rate of 80 ml / min, and maintaining for 2 hours; replacing the introduced ammonia with carbon dioxide at a flow rate of 80 ml / min, and maintaining for 0.2 hours, and then cooling the carbon dioxide to room temperature to obtain a viscose-based carbon fiber;

[0045] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent in a mass ratio of 1:2.2:2.2, wherein the mass ratio of boric acid to ethanol is 1:120, and adding ammonia water to adjust the pH value to 5 to obtain an auxiliary material A solution;

[0046] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution at a mass ratio of 1:2, heating at 80° C. for 4 h, and filtering to obtain a solid;

[0047] 4) placing the product of step 3 into a vacuum tube furnace, heating at 120° C. for 2 h under nitrogen protection, then heating to 1200° C. and heat treating for 5 h to obtain pretreated carbon fiber;

[0048] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:14:8:8, wherein the mass ratio of zirconium nitrate to deionized water is 12:100; stirring evenly at 90° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 6:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.6 to obtain an auxiliary material B solution;

[0049] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:110:8:8, and then placed in an oven for heating for 6 hours to cross-link and solidify to obtain a mixed gel;

[0050] 7) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 900° C. for 7 h, and then heated to 2000° C. for 0.5 h to obtain a viscose-based short fiber thermal insulation composite material.

[0051] Embodiment 4:

[0052] 1) soaking the viscose fiber in water at 90°C for 1 hour, drying, and then soaking in a 5wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60°C for 2 hours, drying, placing the dried product in a tubular furnace, evacuating, heating to 650°C, introducing water vapor at a flow rate of 100 ml / min, and maintaining for 1 hour; replacing the introduced water vapor with ammonia, heating to 900°C, with a flow rate of 100 ml / min, and maintaining for 2 hours; replacing the introduced ammonia with carbon dioxide at a flow rate of 100 ml / min, and maintaining for 0.2 hours, and then cooling to room temperature while maintaining the introduction of carbon dioxide to obtain a viscose-based carbon fiber;

[0053] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent in a mass ratio of 1:2.5:2.5, wherein the mass ratio of boric acid to ethanol is 1:150, adding ammonia water to adjust the pH value to 6, to obtain an auxiliary material A solution;

[0054] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing the short fibers with the auxiliary material A solution at a mass ratio of 1:2.5, heating at 90° C. for 5 h, and filtering to obtain a solid;

[0055] 4) placing the product of step 3 into a vacuum tube furnace, heating at 150° C. for 2 h under nitrogen protection, then heating to 1200° C. and heat treating for 5 h to obtain pretreated carbon fiber;

[0056] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:15:10:10, wherein the mass ratio of zirconium nitrate to deionized water is 15:100; stirring evenly at 90° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 6:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.8 to obtain an auxiliary material B solution;

[0057] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed uniformly in a mass ratio of 100:120:10:10, and then placed in an oven for heating for 6 hours to cross-link and cure to obtain a mixed gel;

[0058] 7) Place the mixed gel in a high temperature furnace, under nitrogen protection, and heat at 900°C for 7 hours, then raise the temperature to

[0059] After heating at 2000℃ for 1h, a viscose-based short fiber thermal insulation composite material was obtained.

[0060] Comparative Example 1 (without pretreatment)

[0061] 1) placing the viscose fiber in a tube furnace, evacuating the vacuum, heating to 900° C., maintaining the temperature for 2 h, and then cooling to room temperature to obtain a viscose-based carbon fiber;

[0062] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent in a mass ratio of 1:2.2:2.2, wherein the mass ratio of boric acid to ethanol is 1:120, and adding ammonia water to adjust the pH value to 5 to obtain an auxiliary material A solution;

[0063] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution at a mass ratio of 1:2, heating at 80° C. for 4 h, and filtering to obtain a solid;

[0064] 4) placing the product of step 3 into a vacuum tube furnace, heating at 120° C. for 2 h under nitrogen protection, then heating to 1200° C. and heat treating for 5 h to obtain pretreated carbon fiber;

[0065] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:14:8:8, wherein the mass ratio of zirconium nitrate to deionized water is 12:100; stirring evenly at 90° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 6:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.6 to obtain an auxiliary material B solution;

[0066] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:110:8:8, and then placed in an oven for heating for 6 hours to cross-link and solidify to obtain a mixed gel;

[0067] 7) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 900° C. for 7 h, and then heated to 2000° C. for 0.5 h to obtain a viscose-based short fiber thermal insulation composite material.

[0068] Comparative Example 2 (without boron carbide coating)

[0069] 1) soaking the viscose fiber in 90°C water for 3 hours, drying, and then soaking it in a 6wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60°C for 3 hours, drying, placing the dried product in a tubular furnace, evacuating, heating to 650°C, introducing water vapor at a flow rate of 80 ml / min, and maintaining for 1 hour; replacing the introduced water vapor with ammonia, heating to 900°C, with a flow rate of 80 ml / min, and maintaining for 2 hours; replacing the introduced ammonia with carbon dioxide at a flow rate of 80 ml / min, and maintaining for 0.2 hours, and then cooling the carbon dioxide to room temperature to obtain a viscose-based carbon fiber;

[0070] 2) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, placing them in a vacuum tube furnace, heating them at 120° C. for 2 h under nitrogen protection, and then heating them to 1200° C. for heat treatment for 5 h to obtain carbon fibers;

[0071] 3) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:14:8:8, wherein the mass ratio of zirconium nitrate to deionized water is 12:100; stirring evenly at 90° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 6:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.6 to obtain an auxiliary material B solution;

[0072] 4) The carbon fiber in step 2, auxiliary material B solution, ethyl orthosilicate and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:110:8:8, and then placed in an oven for heating for 6 hours to cross-link and solidify to obtain a mixed gel;

[0073] 5) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 900° C. for 7 h, and then heated to 2000° C. for 0.5 h to obtain a viscose-based short fiber thermal insulation composite material.

[0074] Comparative Example 3 (2,2-dihydroxybiphenyl is not added to auxiliary material A)

[0075] 1) soaking the viscose fiber in 90°C water for 3 hours, drying, and then soaking it in a 6wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60°C for 3 hours, drying, placing the dried product in a tubular furnace, evacuating, heating to 650°C, introducing water vapor at a flow rate of 80 ml / min, and maintaining for 1 hour; replacing the introduced water vapor with ammonia, heating to 900°C, with a flow rate of 80 ml / min, and maintaining for 2 hours; replacing the introduced ammonia with carbon dioxide at a flow rate of 80 ml / min, and maintaining for 0.2 hours, and then cooling the carbon dioxide to room temperature to obtain a viscose-based carbon fiber;

[0076] 2) dispersing boric acid and polyvinyl alcohol in an ethanol solvent at a mass ratio of 1:2.2, wherein the mass ratio of boric acid to ethanol is 1:120, and adding ammonia water to adjust the pH value to 5 to obtain an auxiliary material A solution;

[0077] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution at a mass ratio of 1:2, heating at 80° C. for 4 h, and filtering to obtain a solid;

[0078] 4) placing the product of step 3 into a vacuum tube furnace, heating at 120° C. for 2 h under nitrogen protection, then heating to 1200° C. and heat treating for 5 h to obtain pretreated carbon fiber;

[0079] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:14:8:8, wherein the mass ratio of zirconium nitrate to deionized water is 12:100; stirring evenly at 90° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 6:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.6 to obtain an auxiliary material B solution;

[0080] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:110:8:8, and then placed in an oven for heating for 6 hours to cross-link and solidify to obtain a mixed gel;

[0081] 7) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 900° C. for 7 h, and then heated to 2000° C. for 0.5 h to obtain a viscose-based short fiber thermal insulation composite material.

[0082] Comparative Example 4 (auxiliary material B without adding polyethyleneimine)

[0083] 1) soaking the viscose fiber in 90°C water for 3 hours, drying, and then soaking it in a 6wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60°C for 3 hours, drying, placing the dried product in a tubular furnace, evacuating, heating to 650°C, introducing water vapor at a flow rate of 80 ml / min, and maintaining for 1 hour; replacing the introduced water vapor with ammonia, heating to 900°C, with a flow rate of 80 ml / min, and maintaining for 2 hours; replacing the introduced ammonia with carbon dioxide at a flow rate of 80 ml / min, and maintaining for 0.2 hours, and then cooling the carbon dioxide to room temperature to obtain a viscose-based carbon fiber;

[0084] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent in a mass ratio of 1:2.2:2.2, wherein the mass ratio of boric acid to ethanol is 1:120, and adding ammonia water to adjust the pH value to 5 to obtain an auxiliary material A solution;

[0085] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution at a mass ratio of 1:2, heating at 80° C. for 4 h, and filtering to obtain a solid;

[0086] 4) placing the product of step 3 into a vacuum tube furnace, heating at 120° C. for 2 h under nitrogen protection, then heating to 1200° C. and heat treating for 5 h to obtain pretreated carbon fiber;

[0087] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:14:8:8, wherein the mass ratio of zirconium nitrate to deionized water is 12:100; stirring evenly at 90° C. to obtain a zirconium sol; dispersing a phenolic resin in ethanol to obtain a phenolic resin mixed solution, wherein the mass ratio of the phenolic resin to the ethanol is 6:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.6 to obtain an auxiliary material B solution;

[0088] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:110:8:8, and then placed in an oven for heating for 6 hours to cross-link and solidify to obtain a mixed gel;

[0089] 7) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 900° C. for 7 h, and then heated to 2000° C. for 0.5 h to obtain a viscose-based short fiber thermal insulation composite material.

[0090] Comparative Example 5 (pretreatment without oxidation)

[0091] 1) soaking the viscose fiber in water at 90° C. for 3 hours, drying, and then soaking in a 6wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60° C. for 3 hours, drying, placing the dried product in a tubular furnace, evacuating, introducing ammonia, heating to 900° C., the flow rate of the ammonia is 80 ml / min, and maintaining for 2 hours; replacing the introduced ammonia with carbon dioxide, the flow rate of the carbon dioxide is 80 ml / min, and maintaining for 0.2 hours, and then cooling to room temperature while continuing to introduce carbon dioxide to obtain a viscose-based carbon fiber;

[0092] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent in a mass ratio of 1:2.2:2.2, wherein the mass ratio of boric acid to ethanol is 1:120, and adding ammonia water to adjust the pH value to 5 to obtain an auxiliary material A solution;

[0093] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution at a mass ratio of 1:2, heating at 80° C. for 4 h, and filtering to obtain a solid;

[0094] 4) placing the product of step 3 into a vacuum tube furnace, heating at 120° C. for 2 h under nitrogen protection, then heating to 1200° C. and heat treating for 5 h to obtain pretreated carbon fiber;

[0095] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:14:8:8, wherein the mass ratio of zirconium nitrate to deionized water is 12:100; stirring evenly at 90° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 6:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.6 to obtain an auxiliary material B solution;

[0096] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:110:8:8, and then placed in an oven for heating for 6 hours to cross-link and solidify to obtain a mixed gel;

[0097] 7) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 900° C. for 7 h, and then heated to 2000° C. for 0.5 h to obtain a viscose-based short fiber thermal insulation composite material.

[0098] Comparative Example 6 (No carbonized nitrogen layer is formed by pretreatment)

[0099] 1) soaking the viscose fiber in water at 90° C. for 3 hours, drying, and then soaking in a 6wt% diammonium hydrogen phosphate aqueous solution at a temperature of 60° C. for 3 hours, drying, placing the dried product in a tubular furnace, evacuating, heating to 650° C., introducing water vapor at a flow rate of 80 ml / min, and maintaining for 1 hour; replacing the introduced water vapor with ammonia, heating to 900° C. at a flow rate of 80 ml / min, maintaining for 2 hours, and then cooling to room temperature to obtain a viscose-based carbon fiber;

[0100] 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent in a mass ratio of 1:2.2:2.2, wherein the mass ratio of boric acid to ethanol is 1:120, and adding ammonia water to adjust the pH value to 5 to obtain an auxiliary material A solution;

[0101] 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution at a mass ratio of 1:2, heating at 80° C. for 4 h, and filtering to obtain a solid;

[0102] 4) placing the product of step 3 into a vacuum tube furnace, heating at 120° C. for 2 h under nitrogen protection, then heating to 1200° C. and heat treating for 5 h to obtain pretreated carbon fiber;

[0103] 5) Dispersing zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol in deionized water at a mass ratio of 100:14:8:8, wherein the mass ratio of zirconium nitrate to deionized water is 12:100; stirring evenly at 90° C. to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol at a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 6:100; mixing the zirconium sol and the phenolic resin mixed solution at a mass ratio of 1:1.6 to obtain an auxiliary material B solution;

[0104] 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate, and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:110:8:8, and then placed in an oven for heating for 6 hours to cross-link and solidify to obtain a mixed gel;

[0105] 7) The mixed gel was placed in a high-temperature furnace, protected by nitrogen, heated at 900° C. for 7 h, and then heated to 2000° C. for 0.5 h to obtain a viscose-based short fiber thermal insulation composite material.

[0106] Test Data

[0107] In the embodiments and comparative examples of the present invention, the process is adjusted in the comparative examples to demonstrate the influence of various process parameters on product performance. The product prepared by the method of the present invention has good thermal insulation performance and good mechanical strength.

[0108] Thermal conductivity: Place the sample in an intelligent double-plate thermal conductivity tester to test the thermal conductivity of the sample at room temperature.

[0109] Compressive strength: Load the sample at a speed of 10 mm / min. When the sample is compressed and deformed by 5%, the load is recorded as the failure load P1.

[0110] Compressive strength calculation formula: A = P1 / S;

[0111] A is the compressive strength of the sample, MPa; P1 is the breaking load of the sample, unit N; S is the compressive area of ​​the sample, unit mm 2 .

[0112] The test results are shown in Table 1 below:

[0113] Table 1

[0114] <![CDATA[Density (g / cm 3 )]]> Thermal conductivity (W / m·K) Compressive strength(MPa) Example 1 0.182 0.136 4.02 Example 2 0.185 0.137 4.10 Example 3 0.191 0.134 4.08 Example 4 0.179 0.135 4.06 Comparative Example 1 0.175 0.105 3.65 Comparative Example 2 0.190 0.192 3.20 Comparative Example 3 0.185 0.176 3.85 Comparative Example 4 0.180 0.180 3.75 Comparative Example 5 0.188 0.186 3.90 Comparative Example 6 0.183 0.195 3.75

[0115] By comparing the embodiments and comparative examples, it can be seen that the mechanical strength and dispersion performance of carbon fiber affect the mechanical properties and thermal insulation performance of the product. The higher the mechanical strength of the fiber and the more uniform the dispersion, the better the compressive resistance of the product. Reducing the aggregation of carbon fiber is also beneficial to reducing thermal conductivity, that is, improving thermal insulation performance. Referring to comparative examples 1, 5, and 6, it can be seen that pre-treating the fiber can effectively improve the mechanical strength and dispersion performance of the fiber; and referring to comparative examples 2 and 3, it can be seen that the boron nitride coating of the product and 2,2-dihydroxybiphenyl in auxiliary material A have obvious effects on the performance of the product. Referring to comparative example 4, it can be seen that in auxiliary material B, polyethyleneimine has an effect on the performance of the product; the product obtained by the present invention, by high-temperature oxidation of viscose fiber under water vapor, generating oxidized groups on the surface of viscose fiber, thereby improving the activation efficiency of amino groups on its surface at high temperature by ammonia, and then the nitrogen-containing groups and the subsequent addition of carbon dioxide at high temperature The carbonized nitrogen groups can improve the surface activity of the fiber and at the same time improve the mechanical strength of the fiber; 2,2-dihydroxybiphenyl can form a stable high-temperature protective layer of boron carbide on the surface of the pretreated carbon fiber at high temperature, thereby reducing the degradation rate of the carbon fiber during subsequent high-temperature carbonization, protecting the carbon fiber and providing excellent mechanical properties, and the presence of boron carbide can also effectively improve the interfacial bonding state of the fiber and the zirconium dioxide ceramic collective; the charge adsorption capacity of polyethyleneimine can disperse the carbon fiber more evenly during the dispersion process, thereby improving the dispersion performance of the carbon fiber in the gel and improving the mechanical properties of the material, and the chopped carbon fiber and ceramic powder can increase the packing density of the gel, while the phenolic resin and polyethyleneimine are cracked into porous carbon during the high-temperature carbonization process, thereby improving the density and strength of the thermal insulation material while improving the thermal insulation performance.

[0116] Although the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention.

Claims

1. A method for preparing a viscose-based short fiber thermal insulation composite material, It is characterized in that The method comprises: 1) pretreating the viscose fiber, then placing the treated viscose fiber in a tubular furnace, evacuating, heating, introducing water vapor, and keeping the temperature; replacing the introduced water vapor with introducing ammonia, continuing to increase the temperature, and keeping the temperature; replacing the introduced ammonia with introducing carbon dioxide, keeping the temperature, and then cooling to room temperature to obtain a viscose-based carbon fiber; 2) dispersing boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl in an ethanol solvent, adding ammonia water to adjust the pH value, and obtaining an auxiliary material A solution; 3) chopping the viscose-based carbon fiber in step 1 to obtain short fibers, then mixing with the auxiliary material A solution, heating and filtering to obtain a solid; 4) placing the product of step 3 into a vacuum tube furnace and heat treating it under nitrogen protection to obtain pretreated carbon fiber; 5) dispersing soluble zirconium salt, oxalic acid, polyvinyl alcohol and glycerol in deionized water, stirring evenly to obtain zirconium sol; dispersing phenolic resin and polyethyleneimine in ethanol to obtain a phenolic resin mixed solution; mixing the zirconium sol and the phenolic resin mixed solution to obtain an auxiliary material B solution; 6) The pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate and dimethyldiethoxysilane are mixed evenly, placed in an oven for heating, and cross-linked and cured to obtain a mixed gel; 7) placing the mixed gel in a high-temperature furnace, protecting it with nitrogen, and subjecting it to heat treatment to obtain a viscose-based short fiber thermal insulation composite material.

2. The method for preparing the viscose-based short fiber thermal insulation composite material according to claim 1, Its characteristics are: The pretreatment process in step 1 includes soaking the viscose fiber in 90-100° C. water for 0.5-3 hours, drying, and then soaking in 50-70° C. 3-6wt% diammonium hydrogen phosphate aqueous solution for 0.5-3 hours and drying.

3. The method for preparing the viscose-based short fiber thermal insulation composite material according to claim 1, Its characteristics are: In the step 1, the treated viscose fiber is placed in a tubular furnace, evacuated, heated to 600-700° C., and water vapor is introduced at a flow rate of 50-100 ml / min for 1-2 hours; the introduced water vapor is replaced by ammonia, the temperature is raised to 850-900° C., the flow rate of ammonia is 50-100 ml / min, and the temperature is maintained for 2-4 hours; the introduced ammonia is replaced by carbon dioxide at a flow rate of 50-100 ml / min for 0.2-0.5 hours, and then the carbon dioxide is kept introduced and cooled to room temperature to obtain viscose-based carbon fiber.

4. The method for preparing the viscose-based short fiber thermal insulation composite material according to claim 1, Its characteristics are: In the step 2, boric acid, polyvinyl alcohol and 2,2-dihydroxybiphenyl are dispersed in an ethanol solvent at a mass ratio of 1:2-2.5:2-2.5, wherein the mass ratio of boric acid to ethanol is 1:100-150, and ammonia water is added to adjust the pH value to 4-6 to obtain an auxiliary material A solution.

5. The method for preparing the viscose-based short fiber thermal insulation composite material according to claim 1, Its characteristics are: In the step 3, the short fibers are mixed with the auxiliary material A solution in a mass ratio of 1:1.5-3, heated at 70-90° C. for 3-6 hours, and filtered to obtain a solid.

6. The method for preparing the viscose-based short fiber thermal insulation composite material according to claim 1, Its characteristics are: In the step 4, the product of step 3 is placed in a vacuum tube furnace, heated at 100-150° C. for 1-2 hours under nitrogen protection, and then heated to 1000-1200° C. and heat treated for 4-6 hours to obtain pretreated carbon fiber.

7. The method for preparing the viscose-based short fiber thermal insulation composite material according to claim 1, Its characteristics are: In the step 5, zirconium nitrate, oxalic acid, polyvinyl alcohol and glycerol are dispersed in deionized water in a mass ratio of 100:10-15:5-10:5-10, wherein the mass ratio of zirconium nitrate to deionized water is 10-15:100; the mixture is stirred at 80-90°C to obtain a zirconium sol; phenolic resin and polyethyleneimine are dispersed in ethanol in a mass ratio of 10:1 to obtain a phenolic resin mixed solution, wherein the mass ratio of phenolic resin to ethanol is 3-6:100; the zirconium sol and the phenolic resin mixed solution are mixed in a mass ratio of 1:1.5-2 to obtain an auxiliary material B solution.

8. The method for preparing the viscose-based short fiber thermal insulation composite material according to claim 1, Its characteristics are: In the step 6, the pretreated carbon fiber of step 4, auxiliary material B solution, ethyl orthosilicate and dimethyldiethoxysilane are mixed evenly in a mass ratio of 100:100-120:5-10:5-10, and then placed in an oven for heating for 2-6 hours to cross-link and cure to obtain a mixed gel.

9. The method for preparing the viscose-based short fiber thermal insulation composite material according to claim 1, Its characteristics are: In step 7, the mixed gel is placed in a high-temperature furnace, protected by nitrogen, heated at 800-900° C. for 5-7 hours, and then heated to 2000-2200° C. for 0.5-1 hour to obtain a viscose-based short fiber thermal insulation composite material.

10. A viscose-based short fiber thermal insulation composite material, Its characteristics are: The material is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Process for preparing biomass porous nitrogen-doped carbon material and fabrication method of supercapacitor electrode

    CN105788876A

  • Zirconium diboride-based composite material toughened by colloid-dispersed chopped carbon fibers and preparation method thereof

    CN105906360A

  • Preparation method of ZrB2 coating on carbon fiber surface

    CN110409170A

  • Preparation method of ZrB2-SiBNC composite coating on carbon fiber surface

    CN110409172A

  • Antioxidant high-temperature-resistant carbon fiber composite material and preparation method thereof

    CN111517817A