Carbon ceramic brake disc and preparation method thereof
Through chemical vapor deposition and glue treatment technology, the problems of white spots and coating peeling of carbon ceramic brake discs are solved, and the preparation of carbon ceramic brake discs with high adhesion and long life is achieved, and the production cost is reduced.
Patent Information
- Application Number
- CN202411191625.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing carbon ceramic brake discs are prone to white spots during use, causing the silicon carbide ceramic coating to fall off, seriously reducing the service life and high preparation cost.
The chemical vapor deposition method is used to carbon densify the preform of the needle-punched structure of carbon fiber, and then the surface of the carbon fiber brake disc is cloth and molded. The adhesive containing inorganic powder and liquid resin is heat-treated and molded, and finally the seepage is carried out. Silicon treatment to avoid white spot defects and improve the adhesiveness of the coating.
It effectively avoids white spots on the surface of the carbon ceramic brake disc, improves the adhesion of the silicon carbide ceramic coating, extends the service life, and reduces the preparation cost, making the price only 1/4 of the prior art.
Smart Images

Figure BDA0005015268780000091 
Figure BDA0005015268780000101 
Figure BDA0005015268780000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon-ceramic brake discs, and in particular relates to a carbon-ceramic brake disc and a preparation method thereof. Background Art
[0002] As people pay more and more attention to the safety of automobile driving, the importance of automobile brake discs is highlighted. Traditional brake discs are cast iron discs, but cast iron discs have the disadvantages of being not wear-resistant, high in density, heavy in weight, and easy to soften and heat up. Compared with cast iron discs, carbon ceramic brake discs not only have low loss and long service life, but also have strong mechanical properties and more stable braking performance.
[0003] However, white spots often exist on the surface of carbon-ceramic brake discs prepared by existing processes, which causes the silicon carbide ceramic coating on the surface of the disc near the white spots to easily fall off during use, seriously reducing the service life of the carbon-ceramic brake disc. Summary of the invention
[0004] The object of the present invention is to provide a carbon-ceramic brake disc and a preparation method thereof. The carbon-ceramic brake disc provided by the present invention has no white spots on the disc surface, the silicon carbide ceramic coating is not easy to fall off, has a long service life, and has a low production cost.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a carbon ceramic brake disc, comprising the following steps:
[0007] Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform;
[0008] Processing the C / C preform into a C / C brake disc;
[0009] After applying glue on the surface of the C / C brake disc, heat treatment and molding treatment are performed in sequence to obtain a semi-finished product, wherein the glue used for the glue application comprises the following components in percentage by weight: 58-75% of inorganic powder, 15-28% of liquid resin and 10-17% of ethanol, wherein the inorganic powder comprises silicon carbide powder and / or carbon powder;
[0010] The semi-finished product is subjected to siliconizing treatment to obtain the carbon-ceramic brake disc.
[0011] Preferably, the method for preparing the needle-punched structural carbon fiber preform comprises the following steps:
[0012] The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns;
[0013] The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric to obtain a laminated blank, and the laminated blank is needle-punched to obtain a needle-punched structural carbon fiber preform.
[0014] Preferably, the thickness of the laminated body is 18 to 30 mm; the density of the laminated body is 0.58 to 0.63 g / m 3 The density of the acupuncture is 25 needles / cm 2 .
[0015] Preferably, the reducing gas used in the chemical vapor deposition is hydrogen, the flow rate of natural gas is 45-75 SLM, the flow rate of hydrogen is 25-50 SLM, the temperature of the chemical vapor deposition is 1000-1100° C., and the deposition time is ≥160 h.
[0016] Preferably, the density of the C / C preform is ≥1.4 g / m 3 .
[0017] Preferably, the amount of adhesive in the adhesive is 0.52 g / cm 2 .
[0018] Preferably, the heat treatment temperature is 100-120° C. and the time is 60-80 min.
[0019] Preferably, the pressing temperature of the molding process is 260-280° C., the pressing time is 30-45 min, and the pressure is 10-14 MPa.
[0020] Preferably, the siliconizing treatment is a molten siliconizing treatment, the temperature of the molten siliconizing treatment is 1400-1550° C., the holding time is 1-3 hours, and the molten siliconizing treatment is carried out in a protective gas atmosphere.
[0021] The present invention provides a carbon-ceramic brake disc prepared by the preparation method described in the above technical solution.
[0022] The invention provides a method for preparing a carbon ceramic brake disc, comprising the following steps: using natural gas as a carbon source gas, and adopting a chemical vapor deposition method to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform; processing the C / C preform into a C / C brake disc; applying glue on the surface of the C / C brake disc, and then sequentially performing heat treatment and molding treatment to obtain a semi-finished product, wherein the glue used for the glue application comprises the following components in percentage by mass: 58-75% of inorganic powder, 15-28% of liquid resin and 10-17% of ethanol, and the inorganic powder comprises silicon carbide powder and / or carbon powder; and performing siliconization treatment on the semi-finished product to obtain the carbon ceramic brake disc. The preparation method provided by the present invention is to apply glue to the surface of the C / C brake disc by means of glue after the carbon fiber preform is carbon densified by chemical vapor deposition and before siliconization, and then the glue is infiltrated into the interior of the C / C brake disc by heat treatment and molding, and the inorganic powder (silicon carbide powder and / or carbon powder) is bonded to the C / C brake disc by liquid resin to form a whole, and then siliconization is performed, which can effectively avoid the white spots (formed by bubbles) on the surface of the obtained carbon ceramic brake disc, so that the obtained silicon carbide ceramic coating is not easy to fall off and has a long service life. At the same time, the preparation method provided by the present invention only requires applying glue, heat treatment and molding treatment to the surface of the C / C brake disc, and the preparation cost is low. The price of the brake disc produced by the present invention is only 1 / 4 of that of the prior art. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing a carbon ceramic brake disc, comprising the following steps:
[0024] Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform;
[0025] Processing the C / C preform into a C / C brake disc;
[0026] After applying glue on the surface of the C / C brake disc, heat treatment and molding treatment are performed in sequence to obtain a semi-finished product, wherein the glue used for the glue application comprises the following components in percentage by weight: 58-75% of inorganic powder, 15-28% of liquid resin and 10-17% of ethanol, wherein the inorganic powder comprises silicon carbide powder and / or carbon powder;
[0027] The semi-finished product is subjected to siliconizing treatment to obtain the carbon-ceramic brake disc.
[0028] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0029] The invention uses natural gas as a carbon source gas and adopts a chemical vapor deposition method to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform.
[0030] In the present invention, the method for preparing the needle-punched structural carbon fiber preform preferably comprises the following steps:
[0031] The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns;
[0032] The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric to obtain a laminated blank, and the laminated blank is needle-punched to obtain a needle-punched structural carbon fiber preform; the thickness of the laminated blank is 18 to 30 mm; the density of the laminated blank is 0.58 to 0.63 g / m 3 The density of the acupuncture is 25 needles / cm 2 .
[0033] The present invention uses short-cut carbon fiber filaments to prepare a mesh tire, and uses long carbon fiber filaments to prepare a non-woven fabric. In the present invention, the short-cut carbon fiber filaments are preferably short-cut T400-24K carbon fiber filaments. The length of the short-cut carbon fiber filaments is preferably 5 to 10 cm. The present invention has no special requirements for the specific preparation method of the mesh tire. The surface density of the mesh tire is preferably 140 g / cm 2 The long carbon fiber yarn is preferably T400-24K carbon fiber yarn. The present invention has no special requirements on the specific preparation method of the non-woven fabric. The surface density of the non-woven fabric is preferably 380g / cm 2 .
[0034] After obtaining the mesh tire and the non-woven fabric, the present invention lays the mesh tire and the non-woven fabric in a cyclic laying manner of one layer of mesh tire and one layer of non-woven fabric to obtain a laminated body, and needle-punches the laminated body to obtain a needle-punched structural carbon fiber preform. In the present invention, during the laying, the non-woven fabric is preferably used alternately in three directions of 0°, 60° and 90°. The thickness of the laminated body is preferably 18 to 30 mm, more preferably 20 to 25 mm. The density of the laminated body is preferably 0.58 to 0.63 g / m 3 , more preferably 0.59 to 0.61 g / m 3 .
[0035] The present invention uses natural gas as a carbon source gas and adopts a chemical vapor deposition (CVD) method to perform carbon densification on the needle-punched carbon fiber preform to obtain a C / C preform.
[0036] In the present invention, the deposition temperature of the chemical vapor deposition is preferably 1000-1100°C, the natural gas flow rate is preferably 45-75SLM, more preferably 48-70SLM, and further preferably 50-65SLM. The auxiliary gas is preferably ethane, and the flow rate of the auxiliary gas is preferably 20SLM. The reducing gas is preferably hydrogen, and the flow rate of hydrogen is preferably 25-50SLM, and more preferably 30-45SLM. The deposition time is preferably ≥160h. In the present invention, the density of the obtained C / C preform is preferably ≥1.4g / cm 3 .
[0037] After obtaining the C / C preform, the present invention processes the C / C preform into a C / C brake disc. The present invention has no special requirements on the specific implementation of the processing. The shape of the C / C brake disc is preferably annular.
[0038] After obtaining the C / C brake disc, the present invention applies glue to the surface of the C / C brake disc and then performs heat treatment and molding treatment in sequence to obtain a semi-finished product, wherein the glue used for the glue application includes the following components in percentage by mass: 58-75% of inorganic powder, 15-28% of liquid resin and 10-17% of ethanol, and the inorganic powder includes silicon carbide powder and / or carbon powder.
[0039] In terms of percentage by mass, the rubber compound used in the present invention includes 58-75% of inorganic powder, preferably 65-75%, and specifically preferably 65% or 75%. The inorganic powder is preferably silicon carbide powder, or the inorganic powder is preferably silicon carbide powder and carbon powder. When the inorganic powder is preferably silicon carbide powder, in terms of percentage by mass, the inorganic powder is preferably 58-75%. The inorganic powder is preferably silicon carbide powder and carbon powder, and in terms of percentage by mass, the inorganic powder is 10-12% carbon powder and 48-53% silicon carbide powder. In the present invention, the function of the inorganic powder in the rubber compound is to form a silicon carbide ceramic surface, wherein the silicon carbide powder and the carbon powder will form a ceramic surface after siliconization, which has good friction and anti-oxidation properties.
[0040] In terms of mass percentage, the surface coating provided by the present invention includes 15 to 28% of liquid resin, preferably 15 to 18%. The liquid resin is preferably a liquid phenolic resin. In a specific embodiment of the present invention, the liquid phenolic resin is preferably purchased from Shandong Shengquan New Materials Co., Ltd. In the present invention, the role of the liquid resin in the sizing agent is bonding. In terms of mass percentage, the sizing agent provided by the present invention includes 10 to 17% of ethanol, preferably 13 to 16%. In the present invention, the role of ethanol in the sizing agent is a diluent. In the present invention, the preparation method of the sizing agent comprises the following steps: mixing silicon carbide powder, liquid resin and ethanol to obtain the sizing agent. The mixing is preferably carried out in a stirring tank, the mixing is preferably carried out under stirring, the stirring speed is preferably 1000 rpm, and the stirring time is preferably 45 to 60 min.
[0041] The present invention preferably applies glue to one of the surfaces of the C / C brake disc, and then sequentially performs heat treatment and molding treatment; then applies glue to the other surface of the C / C brake disc, and then sequentially performs heat treatment and molding treatment, to finally obtain a semi-finished product. The present invention applies glue to the two surfaces of the C / C brake disc, and then sequentially performs heat treatment and molding treatment with the same operating parameters. When applying glue to any one surface of the C / C brake disc, the amount of glue applied to the rubber is preferably 0.52g / cm 2 . The specific implementation method of the adhesive is preferably spraying. After the adhesive is applied, the present invention sequentially performs heat treatment and molding treatment on the C / C brake disc obtained by the adhesive. The temperature of the heat treatment is preferably 100-120°C, more preferably 105-115°C; the time is preferably 60-80min. The heat treatment is preferably carried out in an oven. The present invention preferably transfers the heat-treated C / C brake disc obtained by the heat treatment to a mold for the molding treatment. The molding treatment is preferably carried out on a press. The pressing temperature of the molding treatment is preferably 260-280°C, the pressing time is preferably 30-45min, and the pressing pressure is preferably 10-14MPa.
[0042] In the present invention, after any one surface of the C / C brake disc is subjected to the adhesive treatment, heat treatment and molding treatment in sequence, the molded product is preferably subjected to surface grinding, and the surface grinding is preferably performed in a machining workshop. In the present invention, the heat-treated surface is preferably ground flat by the grinding.
[0043] In a specific embodiment of the present invention, the specific operation process of obtaining the semi-finished product from the C / C brake disc is: applying glue on any surface (any disc surface) of the C / C brake disc, and then performing heat treatment, molding treatment and surface grinding in sequence; then applying glue on the other surface (the other disc surface) of the C / C brake disc, and then performing heat treatment, molding treatment and surface grinding in sequence.
[0044] After obtaining the semi-finished product, the present invention preferably performs a molding process on the semi-finished product before performing the siliconizing treatment. The molding process preferably includes: opening ventilation grooves on the semi-finished product. The molding process is preferably performed in a machining center.
[0045] After the molding process, the present invention performs siliconization treatment on the semi-finished product after the molding process to obtain the carbon ceramic brake disc. In the present invention, the raw material used for the siliconization treatment is preferably silicon powder, and the siliconization treatment is preferably carried out in a siliconization furnace. The present invention preferably places the silicon powder in a crucible with BN coated on the surface, and then places the semi-finished product on the silicon powder, and then places it in a siliconization furnace for siliconization treatment. In the present invention, the siliconization treatment is preferably a molten siliconization treatment, and the temperature of the molten siliconization treatment is preferably 1400-1550°C, the holding time is preferably 1-3h, and the heating time from room temperature to the temperature of the siliconization treatment is preferably 25-30h. The molten siliconization treatment is carried out in a protective gas atmosphere. The present invention preferably fills the siliconization furnace with a protective gas when the temperature of the siliconization furnace is raised from room temperature to 800°C. The protective gas is preferably nitrogen, and the pressure of the protective gas is preferably 70-85kPa.
[0046] In the present invention, after the siliconizing treatment, the present invention preferably performs surface grinding on the siliconized brake disc to obtain the carbon-ceramic brake disc. In the present invention, the surface grinding is preferably performed in a machining workshop. The present invention preferably performs surface grinding on the siliconized brake disc to remove excess silicon material on the surface, and grinds until ceramic cracks appear.
[0047] The present invention provides a carbon-ceramic brake disc prepared by the preparation method described in the above technical solution.
[0048] The carbon ceramic brake disc prepared by the present invention has no white spot defects on its disc surface, and the obtained silicon carbide ceramic coating is not easy to fall off and has a long service life.
[0049] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0050] Example 1
[0051] This embodiment provides a method for preparing a carbon ceramic brake disc, comprising the following steps:
[0052] (1) Preparation of C / C brake disc: A non-woven fabric was prepared using 1400 cm long T400-24K carbon fiber yarn, and a mesh was prepared using 7 cm long chopped T400-24K carbon fiber yarn. A cyclic laying method of one layer of mesh and one layer of non-woven fabric was adopted, wherein the non-woven fabric was used alternately in three directions of 0°, 60° and 90°, with a laying thickness of 30 mm and a volume density of 0.58-0.63 g / cm 3 Finally, acupuncture was performed with a density of 25 needles / cm 2 , forming a needle-punched carbon fiber preform. The needle-punched carbon fiber preform is then treated with chemical vapor deposition (CVI) at a deposition temperature of 1100°C and a deposition time of 160 hours. The deposition gases are natural gas and hydrogen, with a natural gas flow rate of 75 SLM and a hydrogen flow rate of 50 SLM. The density of the C / C preform reaches 1.4 g / cm 3 The C / C preform with the density reaching the standard after deposition is then processed into a ring-shaped C / C brake disc.
[0053] (2) Preparation of mixed materials: The rubber material used in this embodiment includes the following components in percentage by mass: 75% silicon carbide powder, 15% liquid resin, and 10% ethanol. In this embodiment, the components for preparing the rubber material are weighed according to their percentage by mass, and then the weighed silicon carbide powder, liquid resin, and ethanol are added to a stirring tank and stirred continuously (1000 rpm) for 60 minutes. After the mixed solution obtained by stirring is mixed evenly (no visible lumps), the rubber material is obtained.
[0054] (3) Glue filling A side: Pour the glue prepared in step (2) into a mixing tank, and then spray the glue on the C / C brake disc through a glue filling device. The glue filling amount is 0.52 g / cm 2 .
[0055] (4) Baking: The C / C brake disc after the glue filling in step (3) is transferred to an oven and baked for 80 minutes at a set temperature of 120°C.
[0056] (5) Gluing the A side: Transfer the C / C brake disc baked in step (4) to a mold, and then press it on a press. Set the pressing temperature to 280° C. and the pressing time to 45 minutes.
[0057] (6) Machining and grinding: The brake disc pressed in step (5) is subjected to rubber surface turning using a CNC lathe.
[0058] (7) Glue the B side. The operation is the same as step (3).
[0059] (8) Baking: The operation is the same as step (4).
[0060] (9) Glue the B side. The operation steps are the same as (5).
[0061] (10) Machining and grinding. The operation steps are the same as (6).
[0062] (11) Forming processing: The disc body after turning in step (10) is transferred to a machining center for a series of forming processing such as opening ventilation grooves.
[0063] (12) Siliconizing: Place silicon powder in a crucible coated with BN, place the C / C brake disc to be siliconized obtained in step (11) on the silicon powder, and then transfer the crucible to a siliconizing furnace for melt siliconizing treatment, wherein the maximum temperature of the melt siliconizing treatment is 1550°C, the heating time from room temperature to the maximum temperature of the melt siliconizing treatment is 30 hours, and the maximum temperature holding time is 3 hours. During the heating process, when the room temperature reaches 800°C, nitrogen is filled into the siliconizing furnace, and the nitrogen pressure is 85 kPa.
[0064] (13) Finishing: The brake disc after siliconizing in step (12) is transferred to a machining workshop for surface grinding to remove excess silicon material on the surface, and is ground until ceramic cracks appear to obtain a carbon ceramic brake disc.
[0065] The carbon ceramic brake disc prepared in this embodiment has no white spot defects on its disc surface.
[0066] Example 2
[0067] This embodiment provides a method for preparing a carbon ceramic brake disc, comprising the following steps:
[0068] (2) Preparation of C / C brake disc: A non-woven fabric was prepared using T400-24K carbon fiber yarn with a length of 1400 cm, and a mesh was prepared using short-cut T400-24K carbon fiber yarn with a length of 7 cm. A cyclic laying method of one layer of mesh and one layer of non-woven fabric was adopted, wherein the non-woven fabric was used alternately in three directions of 0°, 60° and 90°, with a laying thickness of 30 mm and a volume density of 0.58-0.63 g / cm 3 Finally, acupuncture was performed with a density of 25 needles / cm 2 , forming a needle-punched carbon fiber preform. The needle-punched carbon fiber preform is then treated with chemical vapor deposition (CVI) at a deposition temperature of 1100°C and a deposition time of 160 hours. The deposition gases are natural gas and hydrogen, with a natural gas flow rate of 75 SLM and a hydrogen flow rate of 50 SLM. The density of the C / C preform reaches 1.4 g / cm 3 The C / C preform with the density reaching the standard after deposition is then processed into a ring-shaped C / C brake disc.
[0069] (2) Preparation of mixed materials: The rubber material used in this embodiment includes the following components in percentage by mass: 12% carbon powder, 53% silicon carbide powder, 18% liquid resin, and 17% ethanol. In this embodiment, the components for preparing the rubber material are weighed according to their percentage by mass, and then the weighed silicon carbide powder, liquid resin, and ethanol are added to a stirring tank and stirred continuously (1000 rpm) for 60 minutes. After the mixed solution obtained by stirring is mixed evenly (no visible lumps), the rubber material is obtained.
[0070] (3) Glue filling A side: Pour the glue prepared in step (2) into a mixing tank, and then spray the glue on the C / C brake disc through a glue filling device. The glue filling amount is 0.52 g / cm 2 .
[0071] (4) Baking: The C / C brake disc after the glue filling in step (3) is transferred to an oven and baked for 80 minutes at a set temperature of 120°C.
[0072] (5) Gluing the A side: Transfer the C / C brake disc baked in step (4) to a mold, and then press it on a press. Set the pressing temperature to 280° C. and the pressing time to 45 minutes.
[0073] (6) Machining and grinding: The brake disc pressed in step (5) is subjected to rubber surface turning using a CNC lathe.
[0074] (7) Glue the B side. The operation is the same as step (3).
[0075] (8) Baking: The operation is the same as step (4).
[0076] (9) Glue the B side. The operation steps are the same as (5).
[0077] (10) Machining and grinding. The operation steps are the same as (6).
[0078] (11) Forming processing: The disc body after turning in step (10) is transferred to a machining center for a series of forming processing such as opening ventilation grooves.
[0079] (12) Siliconizing: Place silicon powder in a crucible coated with BN, place the C / C brake disc to be siliconized obtained in step (11) on the silicon powder, and then transfer the crucible to a siliconizing furnace for melt siliconizing treatment, wherein the maximum temperature of the melt siliconizing treatment is 1550°C, the heating time from room temperature to the maximum temperature of the melt siliconizing treatment is 30 hours, and the maximum temperature holding time is 3 hours. During the heating process, when the room temperature reaches 800°C, nitrogen is filled into the siliconizing furnace, and the nitrogen pressure is 85 kPa.
[0080] (13) Finishing: The brake disc after siliconizing in step (12) is transferred to a machining workshop for surface grinding to remove excess silicon material on the surface, and is ground until ceramic cracks appear to obtain a carbon ceramic brake disc.
[0081] Test Case
[0082] The carbon ceramic brake disc prepared in Example 1 was subjected to performance testing. Test method: in accordance with the group standard for brake discs. The mechanical performance test results are shown in Table 1, and the friction test results are shown in Table 2.
[0083] Table 1 Mechanical properties test results of carbon ceramic brake disc prepared in Example 1
[0084]
[0085] Table 2 Friction performance test results of carbon ceramic brake disc prepared in Example 1
[0086]
[0087]
[0088] As can be seen from Table 1 and Table 2, the preparation method of the carbon ceramic brake disc provided by the present invention, after carbon densification of the carbon fiber preform by chemical vapor deposition, before siliconization, the surface of the C / C brake disc is treated with glue by glue, and then through heat treatment and molding treatment, the glue can be infiltrated into the interior of the C / C brake disc, and the inorganic powder (silicon carbide powder and / or carbon powder) is bonded to the C / C brake disc as a whole by liquid resin, and then siliconization treatment is performed, which can effectively avoid the white spot defects on the surface of the obtained carbon ceramic brake disc (when there are white spot defects, the appearance of the carbon ceramic brake disc cannot be guaranteed, and the white spots on the coating mean that the coating has pits), so that the obtained silicon carbide ceramic coating is not easy to fall off and has a long service life. At the same time, the preparation method provided by the present invention only requires glueing, heat treatment and molding treatment on the surface of the C / C brake disc, and the preparation cost is low.
[0089] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a carbon ceramic brake disc, characterized in that: The following steps are involved: Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform; Processing the C / C preform into a C / C brake disc; After applying glue on the surface of the C / C brake disc, heat treatment and molding treatment are performed in sequence to obtain a semi-finished product, wherein the glue used for the glue application comprises the following components in percentage by weight: 58-75% of inorganic powder, 15-28% of liquid resin and 10-17% of ethanol, wherein the inorganic powder comprises silicon carbide powder and / or carbon powder; The semi-finished product is subjected to siliconizing treatment to obtain the carbon-ceramic brake disc.
2. The preparation method according to claim 1, characterized in that: The method for preparing the needle-punched structural carbon fiber preform comprises the following steps: The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns; The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric to obtain a laminated blank, and the laminated blank is needle-punched to obtain a needle-punched structural carbon fiber preform.
3. The preparation method according to claim 2, characterized in that: The thickness of the laminated body is 18 to 30 mm; the density of the laminated body is 0.58 to 0.63 g / m 3 The density of the acupuncture is 25 needles / cm 2 .
4. The preparation method according to claim 1, characterized in that: The reducing gas used in the chemical vapor deposition is hydrogen, the flow rate of natural gas is 45-75 SLM, the flow rate of hydrogen is 25-50 SLM, the temperature of the chemical vapor deposition is 1000-1100° C., and the deposition time is ≥160 hours.
5. The preparation method according to claim 1 or 4, characterized in that: The density of the C / C preform is ≥1.4 g / m 3 .
6. The preparation method according to claim 1, characterized in that: The amount of adhesive on the adhesive is 0.52 g / cm 2 .
7. The preparation method according to claim 1, characterized in that: The heat treatment is carried out at a temperature of 100 to 120° C. and for a time of 60 to 80 minutes.
8. The preparation method according to claim 1, characterized in that: The pressing temperature of the molding process is 260-280° C., the pressing time is 30-45 min, and the pressure is 10-14 MPa.
9. The preparation method according to claim 1, characterized in that: The siliconizing treatment is a molten siliconizing treatment, the temperature of the molten siliconizing treatment is 1400-1550° C., the holding time is 1-3 hours, and the molten siliconizing treatment is carried out in a protective gas atmosphere.
10. A carbon ceramic brake disc prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Carbon-ceramic coating process of carbon-ceramic composite material brake disc
CN120463534A