Pyridyl perovskite nanocrystalline material and preparation and application thereof

By forming bonds with perovskite surface halogen anions, passivating defects, pyridyl perovskite nanocrystalline materials with high nonlinear optical absorption performance were prepared, solving the problems of low stability and charge transport efficiency of perovskite materials. A significantly improved nonlinear optical performance has been achieved.

CN119080687AActive Publication Date: 2024-12-06TONGJI UNIV

Patent Information

Application Number
CN202411099387.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-12-06
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The long-chain ligand used by existing perovskite nanocrystalline materials during the preparation process leads to surface defects, low stability and low charge transfer efficiency, affecting their nonlinear optical properties.

Method used

Using 4-(aminomethyl)pyridine (PyMA) as the surface ligand, the protonated amino groups form bonds with halogen anions on the perovskite inorganic lattice to passivate the surface defects, and a high nonlinear optical performance was prepared. Absorption properties of pyridyl perovskite nanocrystalline materials.

Benefits of technology

The nonlinear optical absorption performance of perovskite nanocrystals is significantly improved, and the nonlinear absorption coefficient reaches 2 times and 1.3 times that of the original material under 800nm ​​and 515nm lasers, respectively, improving the structural stability and charge transfer efficiency of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080687A_ABST
    Figure CN119080687A_ABST
Patent Text Reader

Abstract

The invention relates to a pyridyl perovskite nanocrystalline material as well as preparation and application thereof, PyMA is used as a surface ligand, effective coordination bonding is performed through an amino group on the PyMA and a defect site on a perovskite inorganic lattice, and the novel perovskite nanocrystalline material is prepared. Compared with the prior art, the nanocrystal material disclosed by the invention shows remarkably enhanced nonlinear optical absorption performance in ultrafast femtosecond laser and different wave band regions, which is derived from the introduction of a PyMA surface ligand, passivates defect sites in the perovskite nanocrystal and improves the structural stability of the perovskite nanocrystal. In addition, the aromatic structure of PyMA promotes regular arrangement of ligands on the surface of the perovskite nanocrystals, improves conductivity and enhances electronic coupling between the nanocrystals. The two factors cooperate to endow the target material with excellent nonlinear absorption performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nonlinear optical materials technology, and relates to a pyridine-based perovskite nanocrystalline material and its preparation and application. Background Technology

[0002] All-inorganic halide perovskite nanocrystals, since the first report of all-inorganic cesium halide perovskites (CsPbX3, X = Cl, Br, I) in 2015 (Protesescu L., Yakunin S., Bodnarchuk MI, et al. Nanocrystals of cesium lead halide perovskites (CsPbX3, X = Cl, Br, and I): Novel optoelectronic materials showing bright emission with wide color gamut. Nano Letters, 2015, 15, 3692-3696.), have become a hot topic in next-generation optoelectronics research due to their inherent rich surface properties and quantum confinement effects at the nanoscale, especially in the development of nonlinear optical materials based on perovskite nanocrystals. For example, Sun et al. prepared a 9 nm-sized CsPbBr3 perovskite nanocrystal using a hot-injection method. When tested with an 800 nm laser, the material exhibited strong two-photon absorption, with a two-photon absorption cross-section reaching 1.2 × 10⁻⁶. 5 GM, thus pioneering the application of all-inorganic perovskite nanocrystals in the field of nonlinear optics for the first time (Wang Y., Li X., Zhao X., et al. Nonlinear absorption and low-threshold multiphoton pumped stimulated emission from all-inorganic perovskite nanocrystals. Nano Letters, 2016, 16, 448-453.).

[0003] Compared to three-dimensional bulk perovskites, perovskite nanocrystals offer significantly improved stability. However, their surfaces still contain numerous defect sites, such as vacancies or dangling bonds, which weaken the quantum yield and affect their photonic performance. Most methods for preparing perovskite nanocrystals utilize oleylamine and oleic acid, whose long molecular chains, hydrophobicity, and steric hindrance effectively enhance nanocrystal stability. However, these long-chain ligands are typically electrically insulating, creating energy barriers that hinder carrier transport within the perovskite nanocrystals. Furthermore, their long chain lengths result in excessively large inter-particle spacing, affecting charge transport between perovskite nanocrystals and at conductive contact layer interfaces, thus reducing carrier mobility—a disadvantage for photonic device development. Therefore, preparing perovskite nanocrystals with sufficient light absorption and excellent charge transport performance is a significant challenge in developing high-performance perovskite-based nonlinear photonic devices.

[0004] The present invention is proposed based on the above background. Summary of the Invention

[0005] The purpose of this invention is to provide a pyridine-based perovskite nanocrystal material, its preparation, and its application. By effectively coordinating and bonding the 4-(aminomethyl)pyridine (PyMA) protonated amino group with the halide anion on the inorganic lattice of perovskite, it acts as a surface ligand anchored on the surface of the perovskite nanocrystal, effectively passivating perovskite defects and obtaining a novel pyridine-based perovskite nanocrystal material with high nonlinear optical absorption performance.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] In a first aspect, the present invention provides a pyridyl perovskite nanocrystal material, which uses PyMA as a surface ligand and is bonded to uncoordinated halide anions in the perovskite through its protonated amino groups.

[0008] Furthermore, the chemical formula of the perovskite is CsPbX3, where Cs is a monovalent inorganic cesium cation, Pb is a divalent metallic lead cation, and X3 is a monovalent halide anion.

[0009] In a second aspect, the present invention provides a method for preparing pyridine-based perovskite nanocrystal materials, comprising the following steps:

[0010] (1) Prepare a lead halide precursor solution by mixing and dissolving lead halide, oleic acid, 1-octadecene, oleylamine and 4-(aminomethyl)pyridine;

[0011] (2) The cesium oleate precursor solution was hotly injected into the lead halide precursor solution, reacted, and then cooled;

[0012] (3) Add a dispersion medium to the cooled reaction product solution in step (2) and centrifuge to obtain perovskite nanocrystals, which is the target product.

[0013] Furthermore, in step (1), the mass ratio of 4-(aminomethyl)pyridine to oleylamine is 0.015 to 0.25:1;

[0014] Furthermore, in step (1), the feed ratio of lead halide, oleic acid, 1-octadecene, and oleylamine is (0.45-0.56) mmol: (1.5-1.8) mL: (12-20) mL: (2.2-3) mL.

[0015] Furthermore, in step (2), the cesium oleate precursor solution is prepared by the following method:

[0016] Weigh out cesium carbonate, oleic acid and 1-octadecene and mix them in a ratio of 162.8 mg: (0.5-0.7) mL: (7-9) mL. Then stir and heat to 110-130°C and vacuum dry for 0.5-1.5 h. Then continue to heat under nitrogen atmosphere to 145-155°C until the solution becomes transparent.

[0017] Furthermore, in step (2), before hot injection, the cesium oleate precursor solution is kept at a temperature of 140-150°C, and the lead halide precursor solution is kept at a temperature of 165-170°C.

[0018] Furthermore, in step (2), before hot injection, the lead halide precursor solution is first heated and degassed at 110-120°C for 0.5-1h, and then heated and degassed at 165-170°C for 10-30min.

[0019] Furthermore, in step (2), the reaction time is 5-8 seconds, and after the reaction is completed, the reaction product solution is quickly placed in an ice bath to cool.

[0020] Furthermore, in step (3), the dispersion medium is methyl acetate, n-hexane, or toluene.

[0021] In a third aspect, the present invention provides an application of pyridine-based perovskite nanocrystals as nonlinear optical absorption materials.

[0022] The perovskite nanocrystals prepared in this invention exhibit excellent nonlinear optical absorption properties. Experimental results show that under 800 nm femtosecond laser excitation, the nonlinear absorption coefficient of this material is twice that of the original perovskite nanocrystals; and under 515 nm laser excitation, it is 1.3 times that of the original nanocrystals (i.e., unmodified PyMA perovskite nanocrystals). Mechanistically, this is attributed to the partial substitution of long-chain oleylamine ligands by PyMA surface ligands, which passivates surface defects, thereby reducing the trap state density, improving the stability of the nanocrystal structure, and promoting the coupling of plasmon excitons within the nanocrystals. Furthermore, the aromaticity of short-chain PyMA also promotes charge transfer between perovskite nanocrystal lattice particles, thus enhancing the nonlinear optical absorption properties of the material. Therefore, the PyMA-modified perovskite nanocrystals exhibit structural stability and highly competitive nonlinear optical absorption performance.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] (1) The method for preparing pyridyl perovskite nanocrystals of the present invention can obtain structurally stable perovskite nanocrystals, which can be applied to the development of various halogen perovskite nanocrystals and has a wide range of applications.

[0025] (2) The preparation method of the pyridine-based perovskite nanocrystal material of the present invention is characterized by easy availability of raw materials, material saving, low cost, and simple preparation process.

[0026] (3) The pyridine-based perovskite nanocrystal material of the present invention has good solubility and can be dispersed in polymers, which facilitates the large-scale preparation of thin film materials.

[0027] (4) The pyridine-based perovskite nanocrystal material produced by this invention exhibits more stable chemical properties compared to the original perovskite nanocrystals. Under 800 nm femtosecond laser light, the nonlinear absorption coefficient of the pyridine-based perovskite nanocrystals is twice that of the original perovskite nanocrystals; under 515 nm femtosecond laser light, the nonlinear absorption coefficient of the modified perovskite nanocrystals is 1.3 times that of the original perovskite nanocrystals, demonstrating excellent development potential in the broadband ultrafast laser time domain. This invention shows that the pyridine-based perovskite nanocrystal material overcomes the disadvantage of low nonlinear optical performance of perovskite materials, providing a new reference for constructing high-performance perovskite-based photonic devices. Attached Figure Description

[0028] Figure 1 This is a schematic diagram of the bonding of the pyridine-based perovskite nanocrystal material prepared in this invention.

[0029] Figure 2X-ray diffraction patterns of the pyridine-based perovskite nanocrystal materials (with different PyMA contents) prepared in this invention and the original perovskite nanocrystal materials.

[0030] Figure 3 Transmission electron microscopy (TEM) images of the pyridine-based perovskite nanocrystals (with different PyMA contents) prepared in this invention and the original perovskite nanocrystals.

[0031] Figure 4 Time-resolved fluorescence spectra of the pyridine-based perovskite nanocrystals (with different PyMA contents) prepared in this invention and the original perovskite nanocrystals.

[0032] Figure 5 The Z-scan curves of the pyridine-based perovskite nanocrystal material and the original perovskite nanocrystal material prepared in this invention under 800 nm and 515 nm femtosecond laser excitation, respectively. Detailed Implementation

[0033] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0034] In the following embodiments, the nonlinear optical absorption properties of pyridine-based perovskite nanocrystals and pristine perovskite nanocrystals under femtosecond laser light in the visible and near-infrared regions were tested using an open-aperture Z-scan device. The laser used in the open-aperture Z-scan device was a Ti:sapphire regenerative amplification laser (Spitfre ACE-35F-2KXP, Spectra-Physics type) manufactured by Newport Semiconductor, Inc., with output wavelengths of 800 nm and 515 nm, a pulse width of 35 fs, and a repetition rate of 1000 Hz.

[0035] Example:

[0036] In this invention, PyMA is used as a perovskite surface ligand. By adjusting the ratio, perovskite nanocrystal materials with different contents of PyMA ligands were prepared and labeled as "0.075PyMA-CsPbBr3", "0.15PyMA-CsPbBr3", and "0.25PyMA-CsPbBr3", respectively. The nonlinear absorption performance of the materials was tested under an open-hole Z-scan device.

[0037] The specific steps for preparing various perovskite nanocrystalline materials are as follows:

[0038] (1) Synthesis of cesium oleate: Weigh 162.8 mg of cesium carbonate, 0.6 mL of oleic acid, and 8 mL of 1-octadecene into a two-necked flask, then stir and heat to 120 °C, and then vacuum dry for 1 h. Then heat to 150 °C under a nitrogen atmosphere until the solution becomes transparent, and wait for use.

[0039] (2) Synthesis of CsPbBr3 perovskite nanocrystals: 0.2 g lead bromide, 1.5 mL oleic acid, 15 mL 1-octadecene, and 3 mL oleylamine were weighed into a two-necked flask, and nitrogen gas was repeatedly purged and released three times. The mixture was then heated to 120 °C and stirred while simultaneously degassing under a vacuum pump for 30 min. After this process, the mixture was heated to 170 °C under a nitrogen atmosphere and stirred for 10 min. When the solution became transparent, a cesium oleate solution at 150 °C was quickly drawn up using a glass syringe and rapidly injected into the mixture in the two-necked flask. After 5 s, the two-necked flask was quickly placed in an ice bath to cool, and the flask was continuously shaken. The solution turned bright yellow-green. After the reaction was complete, 50 mL of methyl acetate was added to the crude mixture, and the mixture was centrifuged at 8000 rpm for 5 min. The supernatant was then removed, and the precipitate was redispersed in 2.5 mL of n-hexane. Another 2.5 mL of methyl acetate was added, and the mixture was centrifuged at 8000 rpm for 2 min. The supernatant was then removed again, and the precipitate was redispersed in 5 mL of n-hexane, and centrifuged at 4000 rpm for 5 min. Finally, the supernatant was removed, and the precipitate was dispersed in toluene solution to obtain CsPbBr3 perovskite nanocrystals.

[0040] (3) Synthesis of pyridyl CsPbBr3 perovskite nanocrystals (PyMA-CsPbBr3): The synthesis method is the same as that for CsPbBr3 perovskite nanocrystals, except that the PyMA ligand content varies relative to the mass of oleylamine added (0.075, 0.15, 0.25). Except for the constant amounts of lead bromide, oleic acid, and 1-octadecene, the amounts of other reagents weighed vary as follows:

[0041] 0.075PyMA-CsPbBr3: 75.3mg PyMA, 2.775mL oleylamine;

[0042] 0.15PyMA-CsPbBr3: 150.6mg PyMA, 2.55mL oleylamine;

[0043] 0.25PyMA-CsPbBr3: 251.1mg PyMA, 2.25mL oleylamine.

[0044] (4) The nonlinear absorption properties of two perovskite nanocrystal materials under 800 nm and 515 nm femtosecond laser irradiation were tested by the open-hole Z-scan method.

[0045] Figure 1 This is a schematic diagram illustrating the bonding of the pyridyl perovskite nanocrystal material prepared according to the present invention. The present invention utilizes PyMA as a surface ligand to bond with uncoordinated halide anions in the perovskite. Figure 1 As shown, PyMA containing amino groups partially replaces the long-chain oleylamine ligand and bonds with uncoordinated bromide anions in the perovskite (negative charge defects caused by the absence of cesium cations) to form novel pyridyl perovskite nanocrystals.

[0046] Figure 2 X-ray diffraction (XRD) patterns of the prepared pyridyl perovskite nanocrystals (with different PyMA contents) and the original perovskite nanocrystals are shown. All samples exhibit three distinct XRD peaks at 15.1°, 21.7°, and 30.7°, corresponding to the (100), (110), and (200) crystal planes of the cubic perovskite nanocrystal structure, respectively. Other weaker XRD peaks are also related to the lattice structure of the perovskite nanocrystals. This indicates that the cubic structure of the perovskite nanocrystals remains intact despite the introduction of the PyMA ligand. This implies that the steric hindrance of PyMA molecules has a relatively minor impact on the crystal structure and morphology during the synthesis of perovskite nanocrystals.

[0047] Figure 3 Transmission electron microscopy (TEM) images of the prepared pyridine-based perovskite nanocrystals (with different PyMA contents) and the original perovskite nanocrystals are shown. Regardless of the presence or amount of PyMA added, all perovskite nanocrystals maintained their complete orthorhombic crystal structure and cubic morphology. The lattice fringes with a spacing of 0.58 nm correspond to the (110) crystal plane of the orthorhombic phase of the CsPbBr3 perovskite nanocrystals. This is consistent with the XRD results, indicating that the introduction of the PyMA ligand did not disrupt the inherent crystal structure of the perovskite nanocrystals. Figure 3 It can also be seen that with the addition and increasing content of PyMA, the cubic size of PyMA-modified CsPbBr3 nanocrystals gradually increases. This indicates that the introduction of PyMA ligands has a significant impact on the nucleation and growth kinetics of nanocrystals during the synthesis of perovskite nanocrystals.

[0048] Figure 4The time-resolved fluorescence spectra of the prepared pyridyl perovskite nanocrystals (with different PyMA contents) and the original perovskite nanocrystals are shown. Compared with the original CsPbBr3 perovskite nanocrystals, the PyMA-modified CsPbBr3 nanocrystals exhibit slower fluorescence decay and longer lifetimes. Furthermore, with increasing PyMA content, the nanocrystal size also increases, weakening the quantum confinement effect and leading to an even longer lifetime. This indicates that the introduction of PyMA ligands provides less steric hindrance compared to long-chain oleylamine ligands, thus offering greater degrees of freedom and flexibility. It can passivate defects inaccessible to long-chain oleylamine, effectively reducing the trap state density and thereby suppressing nonradiative recombination in the perovskite nanocrystals.

[0049] Figure 5 The Z-scan curves of the prepared pyridine-based perovskite nanocrystals and the original perovskite nanocrystals under femtosecond laser excitation at 800 nm and 515 nm, respectively, are shown. Compared with the original CsPbBr3 perovskite nanocrystals, the antisaturation absorption performance of CsPbBr3 modified with PyMA ligands is significantly enhanced. Under 800 nm laser excitation, its nonlinear absorption coefficient β value (β = 231.99 × 10⁻⁶) is significantly higher. -3 cm GW -1 It is a pristine CsPbBr3 nanocrystal (β=117.52×10⁻⁶). -3 cm GW -1 It is nearly twice that of other lasers; under 515nm laser excitation, its nonlinear absorption coefficient β value (β=-129.58×10) is... -3 cm GW -1 It is a pristine CsPbBr3 nanocrystal (β=-96.42×10⁻⁶). -3 cm GW -1 It is 1.3 times that of the original. The reason for this may be attributed to the partial substitution of long alkyl chain ligands by PyMA surface ligands, which passivates surface defects, thereby reducing the trap state density, improving the structural stability of the nanocrystal, promoting the coupling of plasmon excitons inside the nanocrystal, and enhancing the nonlinear optical absorption performance.

[0050] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A pyridine-based perovskite nanocrystalline material, It is characterized in that It consists of PyMA as a surface ligand, which bonds with uncoordinated halide anions in the perovskite through its protonated amino groups.

2. The pyridine-based perovskite nanocrystalline material according to claim 1, It is characterized in that The chemical formula of the perovskite is CsPbX 3 , where Cs is a monovalent inorganic cesium cation, Pb is a divalent metal lead cation, and X 3 It is a halogen monovalent halogen anion.

3. A method for preparing a pyridine-based perovskite nanocrystalline material according to claim 1 or 2, It is characterized in that The following steps are involved: (1) preparing a lead halide precursor solution prepared by mixing and dissolving lead halide, oleic acid, 1-octadecene, oleylamine, and 4-(aminomethyl)pyridine; (2) hot-injecting the cesium oleate precursor solution into the lead halide precursor solution, reacting, and cooling; (3) Adding a dispersion medium to the reaction product solution cooled in step (2) and centrifuging the solution to obtain perovskite nanocrystals, which are the target product.

4. The method for preparing a pyridine-based perovskite nanocrystalline material according to claim 3, It is characterized in that In step (1), the mass ratio of 4-(aminomethyl)pyridine to oleylamine is 0.015-0.25:1; the feed ratio of lead halide, oleic acid, 1-octadecene, and oleylamine is (0.45-0.56) mmol: (1.5-1.8) mL: (12-20) mL: (2.2-3) mL.

5. The method for preparing a pyridine-based perovskite nanocrystalline material according to claim 3, It is characterized in that In step (2), the cesium oleate precursor solution is prepared by the following method: Weigh cesium carbonate, oleic acid and 1-octadecene in a ratio of 162.8 mg: (0.5-0.7) mL: (7-9) mL, mix, then stir and heat to 110-130° C., vacuum dry for 0.5-1.5 h, and then continue to heat to 145-155° C. under a nitrogen atmosphere until the solution becomes transparent.

6. The method for preparing a pyridine-based perovskite nanocrystalline material according to claim 3, It is characterized in that In step (2), before hot injection, the temperature of the cesium oleate precursor solution is maintained at 140-150° C., and the temperature of the lead halide precursor solution is maintained at 165-170° C.

7. The method for preparing a pyridine-based perovskite nanocrystalline material according to claim 3, It is characterized in that In step (2), before hot injection, the lead halide precursor solution is first heated at 110-120° C. and degassed for 0.5-1 h, and then continued to be heated at 165-170° C. and degassed for 10-30 min.

8. The method for preparing a pyridine-based perovskite nanocrystalline material according to claim 3, It is characterized in that In step (2), the reaction time is 5-8 s. After the reaction is completed, the reaction product solution is quickly placed in an ice bath for cooling.

9. The method for preparing a pyridine-based perovskite nanocrystalline material according to claim 3, It is characterized in that In step (3), the dispersion medium is methyl acetate, n-hexane, and toluene.

10. Use of a pyridine-based perovskite nanocrystalline material as claimed in claim 1 or 2 as a nonlinear optical absorption material.

Citation Information

Patent Citations

  • Preparation method of water-soluble perovskite nanocrystal, water-soluble perovskite nanocrystal and application

    CN111777096A

  • Polydentate ligand modified perovskite solar cell and preparation method thereof

    CN116528599A

  • Inorganic halide perovskite nanowires and methods of fabrication thereof

    US20170217785A1

Cited By

  • Hybrid based on perovskite nanocrystal-near-infrared dye molecules as well as preparation method and application of hybrid

    CN120248883A