Metal organic complex and preparation method and application thereof, carbon dioxide-based polyurethane and preparation method and application thereof

A metal organic complex catalyst addresses the challenge of controlling polymerization reactions in heterogeneous catalysts, enabling efficient synthesis of carbon dioxide-based polyurethane with high polycarbonate content and narrow molecular weight distribution for industrial applications.

CN119080806APending Publication Date: 2024-12-06LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411190667.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Heterogeneous catalysts used in the synthesis of polycarbonate polyols from carbon dioxide and epoxy compounds lack clear active sites, making it difficult to control polymerization reactions and achieve efficient, industrial-scale production of polyurethanes with precise molecular weight distribution and high polycarbonate group content.

Method used

A metal organic complex is developed, comprising a metal element and an organic ligand, which acts as a catalyst to catalyze the reaction between carbon dioxide and epoxy compounds, resulting in the synthesis of carbon dioxide-based polyurethane with high reaction efficiency, narrow molecular weight distribution, and recyclable properties.

Benefits of technology

The metal organic complex achieves high polycarbonate group content, narrow molecular weight distribution, low by-product formation, and excellent mechanical properties, making it suitable for industrial production of carbon dioxide-based polyurethane with high breaking strength, elongation, and tear strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080806A_ABST
    Figure CN119080806A_ABST
Patent Text Reader

Abstract

The invention provides a metal organic complex and a preparation method and application thereof, and carbon dioxide-based polyurethane and a preparation method and application thereof, and relates to the technical field of polymers. The metal organic complex provided by the invention belongs to a heterogeneous catalyst, and metal potential is blended through an organic ligand, so that the metal active potential on the metal organic complex can promote ring opening of an epoxy compound and insertion of carbon dioxide to generate carbon dioxide-based polycarbonate; further, the generated carbon dioxide-based polycarbonate reacts with isocyanate to generate carbon dioxide-based polyurethane. The metal organic complex provided by the invention is used as a catalyst for preparing carbon dioxide-based polyurethane, and has the advantages of high reaction efficiency, high polycarbonate group content, narrow molecular weight distribution, few byproducts and recyclability of the metal organic complex. Moreover, the prepared carbon dioxide-based polyurethane is high in breaking strength, high in elongation at break, high in tear strength and excellent in mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymers, and in particular to a metal organic complex and a preparation method and application thereof, and a carbon dioxide-based polyurethane and a preparation method and application thereof. Background Art

[0002] Polyurethane is a linear block copolymer containing hard segments and soft segments. Among them, the main monomers constituting the hard segment of the molecular chain are usually diisocyanates, including diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), etc. The monomers constituting the soft segment are mainly polyols, including polycarbonate diols (PCDL), polyethylene glycol (PEG), polypropylene glycol (PPG) and polytetrahydrofuran (PTMG), etc. Since 1969, when Japanese professor Inoue discovered that carbon dioxide and epoxy compounds can undergo catalytic copolymerization to produce polycarbonate, the synthesis of polymer materials using carbon dioxide as raw material has become an important research direction. The polycarbonate polyols generated by carbon dioxide and epoxy compounds can be used as a substitute for commonly used polyols.

[0003] The core of the development of the synthesis of polycarbonate polyols from carbon dioxide and epoxy compounds is the catalyst, which determines the synthesis efficiency, product selectivity and product molecular weight, and realizes the precise control of the microstructure of the polymer. At present, commonly used catalysts include homogeneous catalysts and heterogeneous catalysts. Compared with homogeneous catalysts, heterogeneous catalysts have the characteristics of low cost, easy preparation and separation, and have advantages in industrial production. Commonly used heterogeneous catalysts mainly include alkyl zinc-multiple active hydrogen systems, metal carboxylates, double metal cyanides, rare earth ternary catalysts and supported catalysts. However, heterogeneous catalysts do not have clear active sites, which brings difficulties to the control of the polymerization reaction. Therefore, it is very important to find a highly efficient and easy to regulate polymer molecular weight distribution heterogeneous catalyst. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a metal organic complex and a preparation method and application thereof, a carbon dioxide-based polyurethane and a preparation method and application thereof. The metal organic complex provided by the present invention is used as a catalyst to catalyze carbon dioxide and an epoxy compound to synthesize a carbon dioxide-based polyurethane, which has the advantages of high reaction efficiency, high polycarbonate group content, narrow molecular weight distribution, less by-products, and the metal organic complex can be recycled.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a metal organic complex, comprising a metal element and an organic ligand, wherein the organic ligand has a structure shown in Formula 1:

[0007]

[0008] wherein any two of R1, R2, R3, R4, R5 and R6 are carboxyl groups, and the rest independently include alkyl groups, aromatic groups, carboxyl groups, amino groups, ester groups or halogen groups;

[0009] The metal element includes one or more of transition metals, third group metals and fourth group metals.

[0010] Preferably, the transition metal includes one or more of iron, cobalt, nickel, copper, zinc, chromium, titanium, ruthenium, manganese and cadmium;

[0011] The third main group metal includes aluminum;

[0012] The fourth group metal includes tin.

[0013] The present invention also provides a method for preparing the metal organic complex described in the above technical scheme, comprising the following steps: mixing a metal source, an organic ligand and a first organic solvent, performing a coordination reaction, and obtaining the metal organic complex; the metal element in the metal source comprises one or more of a transition metal, a third main group metal and a fourth main group metal.

[0014] Preferably, the molar ratio of the organic ligand to the metal element is 1:0.1-10;

[0015] The organic solvent includes lower alcohol and / or amide solvent.

[0016] Preferably, the temperature of the coordination reaction is 20-140° C., and the time is 1-100 h.

[0017] The present invention also provides the use of the metal organic complex described in the above technical solution or the metal organic complex prepared by the preparation method described in the above technical solution as a catalyst in the preparation of carbon dioxide-based polyurethane.

[0018] The present invention also provides a method for preparing a carbon dioxide-based polyurethane, comprising the following steps: mixing a catalyst, a chain transfer agent, an isocyanate and an epoxy compound, and performing a polymerization reaction under a carbon dioxide atmosphere to obtain a carbon dioxide-based polyurethane; the catalyst is the metal organic complex described in the above technical solution or the metal organic complex obtained by the preparation method described in the above technical solution.

[0019] Preferably, the chain transfer agent includes one or more of ethylene glycol, polyethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, polypropylene glycol, glycerol, 1,4-butanediol, terephthalic acid and benzenetricarboxylic acid;

[0020] The epoxy compound structural formula is shown in Formula 2:

[0021] Wherein, R'1 and R'2 independently include halogen, aliphatic group, aromatic group, cycloaliphatic group or heterocyclic group;

[0022] The polymerization reaction is carried out in the absence of a solvent or in the presence of a second organic solvent, wherein the second organic solvent comprises one or more of anisole, dichloromethane, 1,4-dioxane, 1,2-dichloroethane and trifluorotoluene.

[0023] The present invention also provides carbon dioxide-based polyurethane prepared by the preparation method described in the above technical scheme.

[0024] The present invention also provides the use of the carbon dioxide-based polyurethane described in the above technical solution in construction, packaging or medical equipment.

[0025] The metal organic complex provided by the present invention belongs to a heterogeneous catalyst. The metal potential is adjusted by an organic ligand so that the metal active potential on the metal organic complex can promote the ring opening of the epoxy compound and the insertion of carbon dioxide to generate carbon dioxide-based polycarbonate, and then the generated carbon dioxide-based polycarbonate reacts with isocyanate to generate carbon dioxide-based polyurethane. The metal organic complex provided by the present invention is used as a catalyst to catalyze carbon dioxide and epoxy compounds to synthesize carbon dioxide-based polyurethane. The reaction TON (Turnover Number) is above 965, and the reaction efficiency is high; the molar content of carbonate chain segments therein is above 94% (calculated based on the carbon dioxide inserted in the epoxy compound), and the content of polycarbonate groups in the carbon dioxide-based polyurethane is high; the molecular weight (PDI) distribution range of the carbon dioxide-based polyurethane is 1.1-1.3, and the molecular weight distribution is narrow; the content of byproduct cyclic carbonate is below 0.11wt%, the byproduct is small, and the purity of the carbon dioxide-based polyurethane is high. Moreover, the metal organic complex has the advantage of being recyclable. The reaction is a heterogeneous catalyst, and the catalyst can be recovered by centrifugation. Moreover, the prepared carbon dioxide-based polyurethane has high breaking strength, high breaking elongation, high tear strength and excellent mechanical properties.

[0026] The preparation method of the metal organic complex provided by the invention has simple process, simple operation, low cost and is suitable for industrial production.

[0027] The preparation method of the carbon dioxide-based polyurethane provided by the present invention has the advantages of high reaction efficiency, high polycarbonate group content, narrow molecular weight distribution, few by-products, and recyclable metal organic complexes. Moreover, the preparation method provided by the present invention has simple process, simple operation, low cost, and is suitable for industrial production. Moreover, the prepared carbon dioxide-based polyurethane has high breaking strength, high breaking elongation, high tear strength, and excellent mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The X-ray diffraction pattern of the metal organic complex prepared in Example 4;

[0029] Figure 2 is the hydrogen spectrum of the carbon dioxide-based polyurethane prepared in Example 16;

[0030] Figure 3 This is the gel chromatography (GPC) chart of the carbon dioxide-based polyurethane prepared in Example 16. DETAILED DESCRIPTION

[0031] The present invention provides a metal organic complex, comprising a metal element and an organic ligand, wherein the organic ligand has a structure shown in Formula 1:

[0032]

[0033] wherein any two of R1, R2, R3, R4, R5 and R6 are carboxyl groups, and the rest independently include alkyl groups, aromatic groups, carboxyl groups, amino groups, ester groups or halogen groups;

[0034] The metal element includes one or more of transition metals, third group metals and fourth group metals.

[0035] In the present invention, the alkyl group preferably includes methyl or ethyl; the aromatic group preferably includes phenyl or naphthyl; the ester group preferably includes methyl formate, methyl acetate, ethyl formate or ethyl acetate; and the halogen preferably includes fluorine, chlorine, bromine or iodine.

[0036] In the present invention, the organic ligand preferably includes 2-aminoterephthalic acid, 2,3-diaminoterephthalic acid, 2-amino-3-methylterephthalic acid, 2,5-diaminoterephthalic acid, 2,6-diaminoterephthalic acid, 2-amino-5-methylterephthalic acid, 2-amino-3-methylcarboxylate terephthalic acid or terephthalic acid.

[0037] In the present invention, the transition metal preferably includes one or more of iron, cobalt, nickel, copper, zinc, chromium, titanium, ruthenium, manganese and cadmium; the third main group metal preferably includes aluminum; and the fourth main group metal preferably includes tin.

[0038] In the present invention, the molar ratio of the organic ligand to the metal element in the metal organic complex is preferably 1:0.1-10, specifically 1:0.1, 1:0.2, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5 or 1:10.

[0039] In the present invention, the metal organic complex preferably includes one or more of a copper-2-aminoterephthalic acid complex, an iron-2,3-diaminoterephthalic acid complex, a cobalt-2-amino-3-methylterephthalic acid complex, a zinc-2,5-diaminoterephthalic acid complex, a chromium-2,6-diaminoterephthalic acid complex, a tin-2-amino-5-methylterephthalic acid complex, a titanium-2-amino-5-chloroterephthalic acid complex, a ruthenium-2-amino-3-methylformate terephthalic acid complex, a manganese-terephthalic acid complex, an aluminum-2-aminoterephthalic acid complex, a cadmium-2-aminoterephthalic acid complex and a nickel-2-aminoterephthalic acid complex.

[0040] The present invention provides a method for preparing the metal organic complex described in the above technical solution, comprising the following steps: mixing a metal source, an organic ligand and a first organic solvent, and performing a coordination reaction to obtain the metal organic complex.

[0041] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.

[0042] In the present invention, the metal source preferably includes a metal salt, more preferably includes one or more of nitrates, formates, acetates and propionates. In the present invention, the metal in the metal source includes one or more of transition metals, third-group metals and fourth-group metals; the transition metal preferably includes one or more of iron, cobalt, nickel, copper, zinc, chromium, titanium, ruthenium, manganese and cadmium; the third-group metal preferably includes aluminum; the fourth-group metal preferably includes tin. In the present invention, the metal source preferably includes one or more of iron formate, cobalt propionate, nickel formate, copper nitrate, zinc acetate, chromium nitrate, tin formate, titanium nitrate, ruthenium formate, manganese nitrate, aluminum nitrate and cadmium nitrate.

[0043] In the present invention, the molar ratio of the organic ligand to the metal element is preferably 1:0.1-10, specifically preferably 1:0.1, 1:0.2, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5 or 1:10.

[0044] In the present invention, the organic solvent preferably includes lower alcohol and / or amide solvent; the lower alcohol preferably includes one or more of methanol, ethanol and isopropanol; the amide solvent preferably includes N-N dimethylformamide and / or N-N dimethylacetamide. In the present invention, the ratio of the amount of the organic ligand to the volume of the first organic solvent preferably includes 1 mol: 10-100 L.

[0045] The present invention has no particular limitation on the mixing as long as the raw materials can be mixed uniformly.

[0046] In the present invention, the temperature of the coordination reaction is preferably 20-140°C, specifically preferably 20°C, 40°C, 80°C, 120°C or 140°C; the time of the coordination reaction is preferably 1-100h, specifically preferably 1h, 3h, 5h, 7h, 15h, 24h, 48h, 72h, 84h, 96h or 100h; the coordination reaction is preferably carried out in a reactor.

[0047] After completing the coordination reaction, the present invention preferably further comprises: subjecting the reaction obtained by the coordination reaction to solid-liquid separation, washing and drying the obtained solid component to obtain a metal organic complex. The present invention has no special limitation on the solid-liquid separation, and can adopt a solid-liquid separation method well known to those skilled in the art, such as filtration, suction filtration or centrifugal separation. In the present invention, the washing solvent preferably comprises lower alcohols and / or amide solvents; the lower alcohol preferably comprises one or more of methanol, ethanol and isopropanol; the amide solvent preferably comprises NN dimethylformamide and / or NN dimethylacetamide. In the present invention, the drying preferably comprises vacuum drying, and the drying temperature is preferably 40 to 200°C, more preferably 50 to 100°C; the drying time is preferably 4 to 24h, more preferably 5 to 15h.

[0048] The present invention also provides the use of the metal organic complex described in the above technical solution or the metal organic complex prepared by the preparation method described in the above technical solution as a catalyst in the preparation of carbon dioxide-based polyurethane.

[0049] The present invention also provides a method for preparing a carbon dioxide-based polyurethane, comprising the following steps: mixing a catalyst, a chain transfer agent, an isocyanate and an epoxy compound, and performing a polymerization reaction under a carbon dioxide atmosphere to obtain a carbon dioxide-based polyurethane; the catalyst is the metal organic complex described in the above technical solution or the metal organic complex obtained by the preparation method described in the above technical solution.

[0050] In the present invention, the epoxy compound has a structural formula as shown in Formula 2:

[0051] Wherein, R'1 and R'2 independently include halogen, aliphatic group, aromatic group, ester ring group or heterocyclic group; the halogen preferably includes fluorine, chlorine, bromine or iodine; the aliphatic group preferably includes methyl or ethyl; the aromatic group preferably includes phenyl or naphthyl; the ester ring group preferably includes cyclopentanolactone group or cyclohexanolactone group; the heterocyclic group preferably includes pyridyl or pyrrolyl.

[0052] In the present invention, the epoxy compound preferably includes one or more of ethylene oxide, ethylene oxide derivatives, propylene oxide, propylene oxide derivatives, cyclohexene oxide and cyclohexene oxide derivatives; the ethylene oxide derivatives preferably include ethylene oxide chloroethane and / or ethylene oxide bromide; the propylene oxide derivatives preferably include epichlorohydrin and / or epibromohydrin; the cyclohexene oxide derivatives preferably include 4-vinylcyclohexane.

[0053] In the present invention, the isocyanate preferably includes one or more of diphenylmethane diisocyanate, cyclohexane diisocyanate, toluene diisocyanate, methylene diisocyanate and hexamethylene diisocyanate. In the present invention, the molar ratio of the isocyanate to the epoxy compound is preferably 1:0.1-1, more preferably 1:0.3-0.5, and specifically preferably 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:1.

[0054] In the present invention, the mass ratio of the isocyanate to the catalyst is preferably 1 mol: 1 to 4 g, more preferably 1 mol: 1 to 2 g.

[0055] In the present invention, the chain transfer agent preferably includes one or more of ethylene glycol, polyethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, polypropylene glycol, glycerol, 1,4-butylene glycol, terephthalic acid and benzenetricarboxylic acid. In the present invention, the molar ratio of the isocyanate to the chain transfer agent is preferably 1:0.01-0.5, and specifically preferably 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.06, 1:0.08, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45 or 1:0.5.

[0056] The present invention has no special limitation on the mixing, as long as the raw materials can be mixed uniformly; the mixing is preferably carried out in a reaction kettle.

[0057] In the present invention, the polymerization reaction is carried out in the absence of a solvent or in the presence of a second organic solvent, and the second organic solvent includes one or more of anisole, dichloromethane, 1,4-dioxane, 1,2-dichloroethane and trifluorotoluene. In the present invention, the volume ratio of the epoxy compound to the solvent is preferably 1:0-10, more preferably 1:3-5, and specifically preferably 1:0.1, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10.

[0058] In the present invention, the polymerization preferably includes: mixing a catalyst, a chain transfer agent and an isocyanate, heating and evacuating, cooling to room temperature, adding an epoxy compound and a second organic solvent (if there is no solvent, it is not added), using carbon dioxide to replace the gas in the reactor, charging carbon dioxide, and performing a polymerization reaction. In the present invention, the heating temperature is preferably 50 to 150°C, more preferably 70 to 100°C, and specifically preferably 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C 140°C, or 150°C; the vacuum degree of the evacuation is preferably 30 to 100kPa, more preferably 50 to 60kPa, and specifically preferably 30kPa, 40kPa, 50kPa, 60kPa, 70kPa, 80kPa, 90kPa or 100kPa. In the present invention, the pressure of the carbon dioxide is preferably 0.1 to 10 MPa, more preferably 0.1 MPa, 0.5 MPa, 1 MPa, 2 MPa, 3 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa or 10 MPa.

[0059] In the present invention, the polymerization temperature is preferably 40-150°C, and is particularly preferably 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C; the polymerization time is preferably 1-100h, and is particularly preferably 1h, 4h, 10h, 20h, 30h, 40h, 50h, 60h, 70h, 80h, 90h or 100h. The present invention utilizes a metal organic complex as a catalyst to catalyze the polymerization reaction of carbon dioxide and an epoxy compound, first synthesizing a polycarbonate polyol, and then synthesizing a carbon dioxide-based polyurethane.

[0060] After the polymerization reaction is completed, the present invention preferably further comprises drying the reaction solution obtained by the polymerization reaction to obtain a carbon dioxide-based polyurethane. In the present invention, the drying preferably comprises vacuum drying, and the drying temperature is preferably 50 to 100° C., more preferably 80° C.; the present invention has no particular limitation on the drying time, and drying to constant weight is sufficient.

[0061] The present invention provides a carbon dioxide-based polyurethane prepared by the preparation method described in the above technical solution. In the present invention, the content of polycarbonate groups in the carbon dioxide-based polyurethane is preferably 30-98%, more preferably 60-90%; the molecular weight distribution of the carbon dioxide-based polyurethane is preferably 1.1-2.5, more preferably 1.1-1.5. The carbon dioxide-based polyurethane prepared by the present invention has a high content of polycarbonate groups and a narrow molecular weight distribution. The carbon dioxide-based polyurethane has high breaking strength, high elongation at break, high tear strength, and excellent mechanical properties.

[0062] The present invention also provides the use of the carbon dioxide-based polyurethane described in the above technical solution in construction, packaging or medical equipment.

[0063] To further illustrate the present invention, the metal organic complex and its preparation method and application, carbon dioxide-based polyurethane and its preparation method and application provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0064] Example 1

[0065] 2-aminoterephthalic acid and copper nitrate were added to methanol, transferred to a reactor, reacted at 20°C for 1 hour, filtered, and the obtained solid component was washed three times with anhydrous ethanol and dried at 80°C for 4 hours to obtain a metal organic complex. The molar ratio of 2-aminoterephthalic acid to copper nitrate was 1:2, and the ratio of the amount of 2-aminoterephthalic acid to the volume of methanol was 1 mol:10L.

[0066] Example 2

[0067] 2,3-diaminoterephthalic acid and iron formate are added to methanol, transferred to a reactor, reacted at 40°C for 3 hours, filtered, and the obtained solid component is washed three times with isopropanol, and dried at 40°C for 6 hours to obtain a metal organic complex. The molar ratio of 2,3-diaminoterephthalic acid to iron formate is 1:0.1, and the ratio of the amount of 2,3-diaminoterephthalic acid to the volume of methanol is 1 mol:10L.

[0068] Example 3

[0069] 2-amino-3-methylterephthalic acid and cobalt propionate were added to ethanol, transferred to a reactor, reacted at 60°C for 5 hours, filtered, and the obtained solid component was washed three times with NN dimethylacetamide, and dried at 180°C for 12 hours to obtain a metal organic complex. Among them, the molar ratio of 2-amino-3-methylterephthalic acid to cobalt propionate was 1:0.2, and the ratio of the amount of 2-amino-3-methylterephthalic acid to the volume of ethanol was 1 mol:10L.

[0070] Example 4

[0071] 2,5-diaminoterephthalic acid and zinc acetate were added to NN dimethylformamide, transferred to a reactor, reacted at 80°C for 7 hours, filtered, and the obtained solid component was washed with anhydrous ethanol and dried at 80°C for 8 hours to obtain a metal organic complex. The molar ratio of 2,5-diaminoterephthalic acid to zinc acetate was 1:2, and the ratio of the amount of 2,5-diaminoterephthalic acid to the volume of NN dimethylformamide was 1 mol:10L.

[0072] Figure 1 This is the X-ray diffraction diagram of the metal organic complex prepared in Example 4 (denoted as Zn catalyst). From the diagram, it can be seen that the characteristic diffraction peaks and metal diffraction peaks of the metal organic complex are present. In addition, the metal organic complex has a high degree of crystallinity.

[0073] Example 5

[0074] 2,6-diaminoterephthalic acid and chromium nitrate were added to methanol, transferred to a reactor, reacted at 100°C for 15 hours, filtered, and the obtained solid component was washed three times with NN dimethylformamide and dried at 80°C for 10 hours to obtain a metal organic complex. The molar ratio of 2,6-diaminoterephthalic acid to chromium nitrate was 1:2, and the ratio of the amount of 2,6-diaminoterephthalic acid to the volume of methanol was 1 mol:10L.

[0075] Example 6

[0076] 2-amino-5-methylterephthalic acid and tin formate are added to methanol, transferred to a reactor, reacted at 120°C for 24 hours, filtered, and the obtained solid component is washed three times with anhydrous methanol, and dried at 100°C for 12 hours to obtain a metal organic complex. Among them, the molar ratio of 2-amino-5-methylterephthalic acid to tin formate is 1:10, and the ratio of the amount of 2-amino-5-methylterephthalic acid to the volume of methanol is 1 mol:100L.

[0077] Example 7

[0078] 2-amino-5-chloroterephthalic acid and titanium nitrate were added to NN dimethylacetamide, transferred to a reactor, reacted at 140°C for 48 hours, filtered, and the obtained solid component was washed three times with anhydrous ethanol, and dried at 150°C for 14 hours to obtain a metal organic complex. Among them, the molar ratio of 2-amino-5-chloroterephthalic acid to titanium nitrate was 1:2, and the ratio of the amount of 2-amino-5-chloroterephthalic acid to the volume of NN dimethylacetamide was 1 mol: 10L.

[0079] Example 8

[0080] Add 2-amino-3-methyl terephthalic acid and ruthenium formate to methanol, transfer to a reactor, react at 160°C for 60 hours, filter, rinse the obtained solid component three times with anhydrous ethanol, and dry at 80°C for 16 hours to obtain a metal organic complex. Among them, the molar ratio of 2-amino-3-methyl terephthalic acid to ruthenium formate is 1:2, and the ratio of the amount of 2-amino-3-methyl terephthalic acid to the volume of methanol is 1 mol: 10L.

[0081] Example 9

[0082] Add terephthalic acid and manganese nitrate to isopropanol, transfer to a reactor, react at 140°C for 72 hours, filter, wash the obtained solid component three times with anhydrous ethanol, and dry at 80°C for 18 hours to obtain a metal organic complex. The molar ratio of terephthalic acid to manganese nitrate is 1:2, and the ratio of the amount of terephthalic acid to the volume of isopropanol is 1 mol:10L.

[0083] Example 10

[0084] 2-aminoterephthalic acid and aluminum nitrate were added to methanol, transferred to a reactor, reacted at 20°C for 84 hours, filtered, and the obtained solid component was washed three times with anhydrous ethanol and dried at 80°C for 12 hours to obtain a metal organic complex. The molar ratio of 2-aminoterephthalic acid to aluminum nitrate was 1:2, and the ratio of the amount of 2-aminoterephthalic acid to the volume of methanol was 1 mol:10L.

[0085] Embodiment 11

[0086] 2-aminoterephthalic acid and cadmium nitrate were added to methanol, transferred to a reactor, reacted at 100°C for 96 hours, filtered, and the obtained solid component was washed three times with anhydrous ethanol, and dried at 200°C for 12 hours to obtain a metal organic complex. The molar ratio of 2-aminoterephthalic acid to cadmium nitrate was 1:2, and the ratio of the amount of 2-aminoterephthalic acid to the volume of methanol was 1 mol:10L.

[0087] Example 12

[0088] 2-aminoterephthalic acid and nickel formate are added to methanol, transferred to a reactor, reacted at 140°C for 100 hours, filtered, and the obtained solid component is washed three times with anhydrous ethanol and dried at 80°C for 20 hours to obtain a metal organic complex. The molar ratio of 2-aminoterephthalic acid to nickel formate is 1:2, and the ratio of the amount of 2-aminoterephthalic acid to the volume of methanol is 1 mol:10L.

[0089] Embodiment 13

[0090] The metal organic complex prepared in Example 1 (200 mg), ethylene glycol (2 mmol), and diphenylmethane diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 70°C and evacuated to a vacuum degree of 50 kPa, and propylene oxide (100 mmol) and anisole (10 mL) were added after the reactor was cooled to room temperature. Carbon dioxide (0.1 MPa) was introduced after carbon dioxide was replaced, the reactor was heated to 40°C and reacted for 1 h, the reactor was opened, and vacuum dried at 80°C to constant weight to obtain a carbon dioxide-based polyurethane.

[0091] Embodiment 14

[0092] The metal organic complex prepared in Example 2 (100 mg), polyethylene glycol (20 mmol), and cyclohexane diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 50°C and evacuated to a vacuum degree of 50 kPa, and after the reactor was cooled to room temperature, ethylene oxide (100 mmol) and dichloromethane (5 mL) were added, and carbon dioxide (2 MPa) was introduced after carbon dioxide replacement. The reactor was heated to 60°C and reacted for 10 hours. The reactor was opened and vacuum dried at 80°C to constant weight to obtain a carbon dioxide-based polyurethane.

[0093] Embodiment 15

[0094] The metal organic complex prepared in Example 3 (200 mg), 1,3-propylene glycol (4 mmol), and toluene diisocyanate (100 mmol) were added to the reactor, the reactor was heated to 60°C and evacuated to a vacuum degree of 30 kPa, and after the reactor was cooled to room temperature, epichlorohydrin (100 mmol) and 1,4-dioxane (1 mL) were added, and carbon dioxide (3 MPa) was introduced after carbon dioxide replacement. The reactor was heated to 80°C and reacted for 20 hours. The reactor was opened and vacuum dried at 80°C to constant weight to obtain carbon dioxide-based polyurethane.

[0095] Example 16

[0096] The metal organic complex prepared in Example 4 (200 mg), propylene glycol (3 mmol), and methylene diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 80°C and evacuated to a vacuum degree of 50 kPa, and after the reactor was cooled to room temperature, cyclohexane oxide (100 mmol) and 1,2-dichloroethane (2 mL) were added, and carbon dioxide (3 MPa) was introduced after carbon dioxide replacement. The reactor was heated to 100°C and reacted for 4 hours. The reactor was opened and vacuum dried at 80°C to constant weight to obtain a carbon dioxide-based polyurethane.

[0097] Embodiment 17

[0098] The metal organic complex prepared in Example 5 (200 mg), 2,4-terephthalic acid (6 mmol), and hexamethylene diisocyanate (50 mmol) were added to a reactor, and the reactor was heated and evacuated. After the reactor was cooled to room temperature, propylene oxide (100 mmol) and trifluorotoluene (5 mL) were added, and carbon dioxide (5 MPa) was introduced after carbon dioxide replacement. The reactor was heated to 140° C. and reacted for 30 h. The reactor was opened and vacuum dried at 80° C. to constant weight to obtain a carbon dioxide-based polyurethane.

[0099] Embodiment 18

[0100] The metal organic complex prepared in Example 6 (200 mg), 1.2-propylene glycol (50 mmol), and diphenylmethane diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 90°C and evacuated to a vacuum degree of 50 kPa, and propylene oxide (100 mmol) was added after the reactor was cooled to room temperature. Carbon dioxide was replaced with carbon dioxide and then introduced (10 MPa). The reactor was heated to 150°C and reacted for 40 hours. The reactor was opened and vacuum dried at 80°C to constant weight to obtain a carbon dioxide-based polyurethane.

[0101] Embodiment 19

[0102] The metal organic complex prepared in Example 7 (200 mg), polypropylene glycol (50 mmol), and diphenylmethane diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 100°C and evacuated to a vacuum degree of 50 kPa. After the reactor was cooled to room temperature, propylene oxide (10 mmol) was added, and carbon dioxide (10 MPa) was introduced after carbon dioxide replacement. The reactor was heated to 150°C and reacted for 50 hours. The reactor was opened and vacuum dried at 80°C to constant weight to obtain a carbon dioxide-based polyurethane.

[0103] Embodiment 20

[0104] The metal organic complex prepared in Example 8 (200 mg), 1,4-butanediol (50 mmol), and cyclohexane diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 110°C and evacuated to a vacuum degree of 50 kPa, and propylene oxide (100 mmol) was added after the reactor was cooled to room temperature. Carbon dioxide was replaced with carbon dioxide and then introduced (10 MPa). The reactor was heated to 150°C and reacted for 60 hours. The reactor was opened and vacuum dried at 80°C to constant weight to obtain a carbon dioxide-based polyurethane.

[0105] Embodiment 21

[0106] The metal organic complex prepared in Example 9 (200 mg, benzenetricarboxylic acid (50 mmol), toluene diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 120°C and evacuated to a vacuum degree of 60 kPa, and propylene oxide (100 mmol) was added after the reactor was cooled to room temperature. Carbon dioxide (10 MPa) was introduced after carbon dioxide was replaced, the reactor was heated to 150°C and reacted for 70 hours, the reactor was opened, and vacuum dried at 80°C to constant weight to obtain a carbon dioxide-based polyurethane.

[0107] Embodiment 22

[0108] The metal organic complex prepared in Example 10 (200 mg), benzenetricarboxylic acid (50 mmol), and methylene diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 130°C and evacuated to a vacuum degree of 70 kPa, and propylene oxide (100 mmol) was added after the reactor was cooled to room temperature. Carbon dioxide was replaced with carbon dioxide and then introduced (10 MPa). The reactor was heated to 150°C and reacted for 80 hours. The reactor was opened and vacuum dried at 80°C to constant weight to obtain a carbon dioxide-based polyurethane.

[0109] Embodiment 23

[0110] The metal organic complex prepared in Example 11 (200 mg), benzenetricarboxylic acid (50 mmol), and hexamethylene diisocyanate (50 mmol) were added to a reactor, the reactor was heated to 140°C and evacuated to a vacuum degree of 80 kPa. After the reactor was cooled to room temperature, propylene oxide (100 mmol) was added, and carbon dioxide (10 MPa) was introduced after carbon dioxide replacement. The reactor was heated to 150°C and reacted for 90 hours. The reactor was opened and vacuum dried at 80°C to constant weight to obtain carbon dioxide-based polyurethane.

[0111] Embodiment 24

[0112] The metal organic complex prepared in Example 12 (200 mg), benzenetricarboxylic acid (50 mmol), and diphenylmethane diisocyanate (100 mmol) were added to a reactor, the reactor was heated to 150°C and evacuated to a vacuum degree of 90 kPa, and propylene oxide (100 mmol) was added after the reactor was cooled to room temperature. Carbon dioxide (10 MPa) was introduced after carbon dioxide was replaced, the reactor was heated to 150°C and reacted for 100 hours, the reactor was opened, and vacuum dried at 80°C to constant weight to obtain carbon dioxide-based polyurethane.

[0113] Comparative Example 1

[0114] The carbon dioxide-based polyurethane sponge used for insoles prepared in Example 1 of CN118085221A.

[0115] Test Example 1

[0116] (1) Product property test of carbon dioxide-based polyurethane

[0117] Figure 2 is the hydrogen spectrum of the carbon dioxide-based polyurethane prepared in Example 16, Figure 3 This is the gel chromatography (GPC) diagram of the carbon dioxide-based polyurethane prepared in Example 16, Figure 3 The middle curve overlaps with the text information but does not affect the expression of the technical effect.

[0118] The molar amount of inserted carbon dioxide CU and the by-product content can be obtained by nuclear magnetic hydrogen spectrum analysis, and the calculation formula is shown in Formula 1; the molecular weight distribution PDI is obtained by gel chromatography (TOSOH HLC-8230GPC) test, and the calculation formula is shown in Formula 2; the turnover number TON = m (product) / m (catalyst), and the test results are shown in Table 1.

[0119] CU=(A 5.0 +A 4.2 -2A 4.58 ) / (A 5.0 +A 4.2 -2A 4.58 +A 3.5 ) Formula 1;

[0120] W PC =(102A 1.5 ) / (58A 1.14 +102A 1.33 +102A 1.5 )Formula 2.

[0121] In formula 1, A 5.0 Represents polycarbonate (1H), A 4.2 Represents polycarbonate (2H), A 4.58 represents cyclic carbonate (1H), A 3.5 represents polyether (2H);

[0122] In formula 2, A 1.5 represents cyclic carbonate (3H), A 1.14 Represents polyether (3H), A 1.33 It represents polycarbonate (3H).

[0123] Table 1 Product properties of carbon dioxide-based polyurethanes prepared in Examples 13 to 24

[0124] CU / % PDI TON By-product content / wt% Embodiment 13 98 1.2 1120 0.1% Embodiment 14 97 1.1 1054 0.08% Embodiment 15 96 1.3 986 0.07% Example 16 94 1.3 978 0.33% Embodiment 17 97 1.3 1153 0.09% Embodiment 18 96 1.2 1038 0.08% Embodiment 19 97 1.3 1023 0.06% Embodiment 20 95 1.3 995 0.12% Embodiment 21 96 1.2 965 0.1% Embodiment 22 94 1.2 1044 0.08% Embodiment 23 95 1.1 1162 0.07% Embodiment 24 96 1.2 1073 0.11%

[0125] As can be seen from Table 1, when the metal organic complex provided by the present invention is used as a catalyst to catalyze carbon dioxide and epoxide compounds to synthesize carbon dioxide-based polyurethane, the reaction turnover number is above 965, and the reaction efficiency is high; the molar content of carbon dioxide inserted into the epoxide is above 94%, and the content of polycarbonate groups in the carbon dioxide-based polyurethane is high; the molecular weight distribution range is 1.1 to 1.3, and the molecular weight distribution of the carbon dioxide-based polyurethane is narrow; the content of by-product cyclic carbonate in the carbon dioxide-based polyurethane is below 0.11wt%, the by-product is small, and the purity of the carbon dioxide-based polyurethane is high.

[0126] (2) Mechanical properties test of CO2-based polyurethane

[0127] Tensile strength and elongation at break: The samples obtained in the embodiments and comparative examples were tested according to the national standard GB / T6344-2008 at a test rate of 500 mm / min. The test results are shown in Table 2.

[0128] Tear strength: Chopping knife specification 101.6mm×19.1mm, 3 test pieces, R (chamfer) 90°, R (width) 12.7mm, clamp distance 75mm, machine speed 500mm / min, until it breaks. The test results are shown in Table 2.

[0129] Table 2 Performance test results

[0130]

[0131]

[0132] As shown in Table 2, the polyurethane of the present invention has a maximum breaking strength of 84.2 MPa, a maximum breaking elongation of 143.7%, and a tear strength of 15.2 kg / cm. These data are better than those of the comparative example. More importantly, the method of the present invention is relatively simple, which simplifies the reaction steps while improving the performance.

[0133] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A metal-organic complex, characterized in that: It includes a metal element and an organic ligand, wherein the organic ligand has a structure shown in Formula 1: wherein any two of R1, R2, R3, R4, R5 and R6 are carboxyl groups, and the rest independently include alkyl groups, aromatic groups, carboxyl groups, amino groups, ester groups or halogen groups; The metal element includes one or more of transition metals, third group metals and fourth group metals.

2. The metal-organic complex according to claim 1, characterized in that The transition metal includes one or more of iron, cobalt, nickel, copper, zinc, chromium, titanium, ruthenium, manganese and cadmium; The third main group metal includes aluminum; The fourth group metal includes tin.

3. The method for preparing the metal organic complex according to claim 1 or 2, characterized in that: The following steps are involved: Mixing a metal source, an organic ligand and a first organic solvent to carry out a coordination reaction to obtain the metal-organic complex; The metal elements in the metal source include one or more of transition metals, third group metals and fourth group metals.

4. The preparation method according to claim 3, characterized in that: The molar ratio of the organic ligand to the metal element is 1:0.1-10; The organic solvent includes lower alcohol and / or amide solvent.

5. The preparation method according to claim 3 or 4, characterized in that: The temperature of the complexing reaction is 20-140° C., and the time is 1-100 hours.

6. Use of the metal organic complex according to any one of claims 1 to 2 or the metal organic complex prepared by the preparation method according to any one of claims 3 to 5 as a catalyst in the preparation of carbon dioxide-based polyurethane.

7. A method for preparing a carbon dioxide-based polyurethane, characterized in that: The following steps are involved: The catalyst, chain transfer agent, isocyanate and epoxy compound are mixed and polymerized under a carbon dioxide atmosphere to obtain a carbon dioxide-based polyurethane; The catalyst is the metal organic complex described in any one of claims 1 to 2 or the metal organic complex prepared by the preparation method described in any one of claims 3 to 5.

8. The preparation method according to claim 7, characterized in that: The chain transfer agent includes one or more of ethylene glycol, polyethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, polypropylene glycol, glycerol, 1,4-butanediol, terephthalic acid and benzenetricarboxylic acid; The epoxy compound structural formula is shown in Formula 2: Wherein, R'1 and R'2 independently include halogen, aliphatic group, aromatic group, cycloaliphatic group or heterocyclic group; The polymerization reaction is carried out in the absence of a solvent or in the presence of a second organic solvent, wherein the second organic solvent comprises one or more of anisole, dichloromethane, 1,4-dioxane, 1,2-dichloroethane and trifluorotoluene.

9. The carbon dioxide-based polyurethane prepared by the preparation method according to claim 7 or 8.

10. Use of the carbon dioxide-based polyurethane according to claim 9 in construction, packaging or medical devices.