Preparation method of phosphite flame retardant
By using alkoxides to replace alcohols in the preparation of phosphite flame retardants and reacting under negative pressure, the problems of low reaction yield and many by-products in the prior art are solved, and efficient and environmentally friendly Preparation method avoids equipment corrosion and environmental pollution.
Patent Information
- Application Number
- CN202411083897.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-12-06
AI Technical Summary
In the existing preparation methods for phosphite-based flame retardants, the transesterification method has low reaction yields and the trichlorophosphite esterification method produces many by-products, including corrosive HCl, which leads to equipment corrosion and environmental pollution.
Using a new reaction path, by adding phosphorus trichloride and catalyst to the enamel reactor, using alkoxide to replace alcohol, the reaction under gradient heating and negative pressure conditions is avoided, and the formation of hydrochloric acid and equipment corrosion is achieved, and environmentally friendly process route.
It improves the reaction yield, reduces the generation of by-products, avoids equipment corrosion, and has a more environmentally friendly process.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardants, and in particular to a method for preparing a phosphite flame retardant. Background Art
[0002] At present, the preparation methods of phosphite antioxidants mainly include ester exchange method, trichlorophosphite esterification method, etc. The reaction equations are as follows: Ester exchange method: P (OR1) 3 + 3R2OH - P (OR2) 3 + 3R1OH OR1 is mainly -OCH3 and -OC2H5, R1 is a low-boiling point small molecular weight aliphatic hydrocarbon, OR2 is mainly -OC n H 2n+1 , R2 is a high-boiling point, high-molecular-weight aliphatic or aromatic hydrocarbon, and the n value is generally between 6 and 18 carbon atoms.
[0003] Phosphite trichloride method: Of these two process technologies, the first process technology has a low reaction yield, while the second process technology has more by-products, including the generation of HCl, which corrodes equipment and also has a relatively low yield. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a phosphite flame retardant, which adopts a new reaction path, has no generation of hydrochloric acid in the reaction product, does not corrode equipment, and is more environmentally friendly.
[0005] To achieve this object, the present invention adopts the following technical solutions: Provided is a method for preparing a phosphite flame retardant, comprising the following steps: Purge the enameled reactor, dropping tank and distillation kettle clean with nitrogen; Add phosphorus trichloride and solvent into the enameled reactor and stir; Adding a catalyst into the enameled reactor; Add alkoxide and solvent into the dropping tank; Gradually add the solution in the dropping tank into the enameled reactor; Start the agitator of the enamel reactor to stir, and perform gradient temperature increase, and control the pressure in the reactor to be negative pressure, wherein the gradient temperature increase does not exceed 60°C to 80°C, and the temperature increase reaction time is 2 to 3h; After the enameled reactor is heated to 60°C to 80°C, it is kept for aging for 3 to 5 hours until the total content of R1ONa, R1OH, R1COOR2 and R1COCl in the reactor is ≤0.1%, and the aging is stopped, wherein R1- and R2- in R1ONa, R1OH, R1COOR2 and R1COCl are aliphatic alcohols and aromatic alcohols with 1 to 8 C atoms; The enameled reactor was gradually cooled to 30-40°C to precipitate NaCl crystals; Filter the salt crystals and wash the salt with a solvent 2 to 3 times, wherein the washing liquid is recovered in the filtrate; The filtrate was added into the distillation kettle, the temperature was gradually raised, and the vacuum was drawn, wherein the pressure gradually dropped from 0 MPa to -0.098 MPa; The front fraction is collected and refluxed into the distillation kettle, and the reflux ratio is controlled to obtain the phosphite product.
[0006] As a preferred embodiment of the method for preparing the phosphite flame retardant, the step of adding the alcohol salt and the solvent into the dropping tank further comprises: adding the alcohol ester corresponding to the alcohol salt into the dropping tank.
[0007] As a preferred embodiment of the preparation method of the phosphite flame retardant, the catalyst is a Lewis acid-matched mixture of one or more of AlCl3, FeCl3, CuCl2, MgCl2, CuCl, TiCl4 and tetrabutyl titanate, or a Lewis acid-matched mixture of one or more of organic amine, sodium hydroxide, potassium hydroxide, sodium alcohol salt, sodium phenolate and diphenyl phosphite.
[0008] As a preferred solution of the preparation method of phosphite flame retardant, the mass of the catalyst is 3-5‰ of the mass of phosphorus trichloride.
[0009] As a preferred solution of the preparation method of phosphite flame retardant, the solvent is ethylene dichloride, toluene, xylene, methylcyclohexane, or corresponding alcohol ester.
[0010] As a preferred scheme for the preparation method of phosphite flame retardant, in the step of starting the enameled reactor agitator for stirring and performing gradient temperature increase, the pressure in the reactor is controlled to be negative pressure, wherein the gradient temperature increase does not exceed 60°C, the temperature increase reaction time is 2h to 3h, and the pressure in the reactor is a slight negative pressure of -0.03 to -0.04MPa.
[0011] As a preferred embodiment of the method for preparing a phosphite flame retardant, after the fore fraction is collected and refluxed into a distillation kettle, the reflux ratio is controlled to obtain a phosphite product, and the method comprises: The solvent is purified by vacuum distillation until the water content of the solvent is ≤1‰ for recycling.
[0012] As a preferred solution of the preparation method of phosphite flame retardant, after the enamel reactor is heated to 60°C, it is kept warm for 3 to 5 hours until the total content of R1ONa, R1OH, R1COOR2 and R1COCl in the reactor is ≤0.1%, and the step of stopping aging includes: Detect the total content of R1ONa, R1OH, R1COOR2 and R1COCl in the enameled reactor.
[0013] Beneficial effects of the present invention: The preparation method of the phosphite flame retardant proposed by the present invention adopts alcohol salt to replace alcohol, and under the catalysis of the catalyst, no corrosive HCl gas is generated in the reaction product, which reduces the corrosion to the equipment and belongs to an environmentally friendly process route. DETAILED DESCRIPTION
[0014] The embodiments of the present disclosure are described in detail below.
[0015] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present disclosure, rather than all of the embodiments. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present disclosure. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present disclosure.
[0016] The present invention adopts a new preparation process of phosphite. Under the catalysis of a catalyst, the reaction equation is as follows: PCl3+3R1ONa——P(OR1)3+3NaCl Alcohol salts or a mixture of alcohol esters and alcohol salts are used to replace alcohols, and the reaction product does not generate corrosive HCl gas, which reduces corrosion to equipment and is an environmentally friendly process route. Among them, R1- and R2- of R1ONa or R1COOR2 can be aliphatic alcohols and aromatic alcohols with 1 to 8 carbon atoms.
[0017] Example 1 Preparation of trimethyl phosphite S1: Purge the enameled reactor, dropping tank and distillation kettle with nitrogen; S2: Add 137.5 kg of phosphorus trichloride and 200 kg of ethylene dichloride solvent into an enameled reactor and stir; S3: Add 3‰ of the mass of phosphorus trichloride into the enameled reactor. S4: Add 189 kg of sodium methanolate and 300 kg of ethylene dichloride solvent into the dropping tank while stirring; S5: gradually adding the solution in the dropping tank to the enameled reactor; S6: Start the agitator of the enamel reactor to stir, and perform gradient temperature increase, and control the pressure in the reactor to be a slight negative pressure of -0.03 to -0.04 MPa, wherein the gradient temperature increase does not exceed 60°C, and the temperature increase reaction time is 2 to 3 hours; S7: After the enameled reactor is heated to 60°C, it is kept warm for 3-5 hours and then sampled for testing. If the total content of CH3ONa and CH3OH in the reactor is ≤0.1%, it is considered that the reaction endpoint has been reached and the aging process is stopped. S8: gradually cooling the enameled reactor to 30-40°C to precipitate NaCl crystals; S9: filtering the salt crystals and washing the salt with a solvent 2 to 3 times, wherein the washing solution is recovered into the filtrate; S10: adding the filtrate into the distillation kettle, gradually increasing the temperature, and evacuating the kettle, wherein the pressure gradually decreases from 0 MPa to -0.098 MPa; S11: The front fraction is collected and refluxed into the distillation kettle, and the reflux ratio is controlled to obtain trimethyl phosphite product.
[0018] S12: Purify the solvent by vacuum distillation until the water content of the solvent is ≤1‰ for recycling.
[0019] Example 2 Preparation of trimethyl phosphite The difference between this embodiment 2 and embodiment 1 is that in step S4, 90 kg of methyl formate and 108 kg of sodium methoxide mixture are used instead of 189 kg of sodium methoxide; The other steps are the same as those in Example 2.
[0020] Example 3 Preparation of triethyl phosphite S1: Purge the enameled reactor, dropping tank and distillation kettle with nitrogen; S2: Add 137.5 kg of phosphorus trichloride and 200 kg of methylcyclohexane solvent into an enameled reactor and stir; S3: Add 3‰ of the mass of phosphorus trichloride into the enameled reactor. S4: Add 238 kg of ethanol sodium salt and 500 kg of methylcyclohexane solvent into the dropping tank while stirring; S5: gradually adding the solution in the dropping tank to the enameled reactor; S6: Start the agitator of the enamel reactor to stir, and perform gradient temperature increase, and control the pressure in the reactor to be a slight negative pressure of -0.03 to -0.04 MPa, wherein the gradient temperature increase does not exceed 80°C, and the temperature increase reaction time is 2 to 3 hours; S7: After the enameled reactor is heated to 80°C, it is kept for aging for 3 to 5 hours, and samples are taken for testing. If the total content of CH3CH2ONa and CH3CH2OH in the reactor is ≤0.1%, it is considered that the reaction endpoint has been reached and the aging is stopped; S8: gradually cooling the enameled reactor to 30-40°C to precipitate NaCl crystals; S9: filtering the salt crystals and washing the salt with a solvent 2 to 3 times, wherein the washing solution is recovered into the filtrate; S10: adding the filtrate into the distillation kettle, gradually increasing the temperature, and evacuating the kettle, wherein the pressure gradually decreases from 0 MPa to -0.098 MPa; S11: The front fraction is collected and refluxed into the distillation kettle, and the reflux ratio is controlled to obtain triethyl phosphite product.
[0021] S12: Purify the solvent by vacuum distillation until the water content of the solvent is ≤1‰ for recycling.
[0022] Example 4 Preparation of triethyl phosphite The difference between this embodiment 4 and embodiment 3 is that in step S4, 132 kg of ethyl acetate and 136 kg of sodium ethoxide mixture are used instead of 238 kg of sodium ethoxide; The other steps are the same as those in Example 3.
[0023] Example 5 Preparation of tributyl phosphite S1: Purge the enameled reactor, dropping tank and distillation kettle with nitrogen; S2: Add 137.5 kg of phosphorus trichloride and 200 kg of toluene solvent into an enameled reactor and stir; S3: Add 3‰ of the mass of phosphorus trichloride into the enameled reactor. S4: Add 336 kg of sodium butanol and 700 kg of toluene solvent into the dropping tank; S5: gradually adding the solution in the dropping tank to the enameled reactor; S6: Start the agitator of the enamel reactor to stir, and perform gradient temperature increase, and control the pressure in the reactor to be a slight negative pressure of -0.03 to -0.04 MPa, wherein the gradient temperature increase does not exceed 80°C, and the temperature increase reaction time is 2 to 3 hours; S7: After the enameled reactor is heated to 80°C, it is kept for aging for 3 to 5 hours. Samples are taken for testing. If the total content of C4H9ONa and C4H9OH in the reactor is ≤0.1%, it is considered that the reaction endpoint has been reached and the aging is stopped. S8: gradually cooling the enameled reactor to 30-40°C to precipitate NaCl crystals; S9: filtering the salt crystals and washing the salt with a solvent 2 to 3 times, wherein the washing solution is recovered into the filtrate; S10: adding the filtrate into the distillation kettle, gradually increasing the temperature, and evacuating the kettle, wherein the pressure gradually decreases from 0 MPa to -0.098 MPa; S11: The front fraction is collected and refluxed into the distillation kettle, and the reflux ratio is controlled to obtain tributyl phosphite product.
[0024] S12: Purify the solvent by vacuum distillation until the water content of the solvent is ≤1‰ for recycling.
[0025] Example 6 Preparation of tributyl phosphite The difference between this embodiment 6 and embodiment 5 is that in step S4, 216 kg of n-butyl butyrate and 192 kg of sodium butoxide mixture are used instead of 336 kg of sodium butoxide salt; The other steps are the same as those in Example 5.
[0026] The above is only for explaining the implementation mode of the present invention and is not intended to limit the present invention. For those skilled in the art, any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention without creative work should be included in the protection scope of the present invention.
Claims
1. A method for preparing a phosphite flame retardant, characterized in that: The following steps are involved: Purge the enameled reactor, dropping tank and distillation kettle clean with nitrogen; Add phosphorus trichloride and solvent into the enameled reactor and stir; Adding a catalyst into the enameled reactor; Add alkoxide and solvent into the dropping tank; Gradually add the solution in the dropping tank into the enameled reactor; Start the agitator of the enamel reactor to stir, and perform gradient temperature increase, and control the pressure in the reactor to be negative pressure, wherein the gradient temperature increase does not exceed 60°C to 80°C, and the temperature increase reaction time is 2 to 3h; After the enameled reactor is heated to 60°C to 80°C, it is kept for aging for 3 to 5 hours until the total content of R1ONa, R1OH, R1COOR2 and R1COCl in the reactor is ≤0.1%, and the aging is stopped, wherein R1- and R2- in R1ONa, R1OH, R1COOR2 and R1COCl are aliphatic alcohols and aromatic alcohols with 1 to 8 C atoms; The enameled reactor was gradually cooled to 30-40°C to precipitate NaCl crystals; Filter the salt crystals and wash the salt with a solvent 2 to 3 times, wherein the washing liquid is recovered in the filtrate; The filtrate was added into the distillation kettle, the temperature was gradually raised, and the vacuum was drawn, wherein the pressure gradually dropped from 0 MPa to -0.098 MPa; The front fraction is collected and refluxed into the distillation kettle, and the reflux ratio is controlled to obtain the phosphite product.
2. The method for preparing the phosphite flame retardant according to claim 1, characterized in that: The step of adding the alkoxide and the solvent into the dropping tank further includes: adding the alcohol ester corresponding to the alkoxide into the dropping tank.
3. The method for preparing the phosphite flame retardant according to claim 1, characterized in that: The catalyst is a Lewis acid-matched mixture of one or more of AlCl3, FeCl3, CuCl2, MgCl2, CuCl, TiCl4 and tetrabutyl titanate, or a Lewis acid-matched mixture of one or more of organic amine, sodium hydroxide, potassium hydroxide, sodium alcoholate, sodium phenolate and diphenyl phosphite.
4. The method for preparing the phosphite flame retardant according to claim 1, characterized in that: The mass of the catalyst is 3-5‰ of the mass of phosphorus trichloride.
5. The method for preparing the phosphite flame retardant according to claim 1, characterized in that: The solvent is ethylene dichloride, toluene, xylene, methylcyclohexane, or corresponding alcohol ester.
6. The method for preparing the phosphite flame retardant according to claim 1, characterized in that: In the step of starting the agitator of the enamel reactor to stir, and performing gradient temperature increase, controlling the pressure in the reactor to be negative pressure, wherein the gradient temperature increase does not exceed 60°C, and the temperature increase reaction time is 2h to 3h, the pressure in the reactor is a slight negative pressure of -0.03 to -0.04MPa.
7. The method for preparing the phosphite flame retardant according to claim 1, characterized in that: After the front fraction is collected and refluxed into the distillation kettle, the reflux ratio is controlled to obtain the phosphite product, and the method comprises: The solvent is purified by vacuum distillation until the water content of the solvent is ≤1‰ for recycling.
8. The method for preparing the phosphite flame retardant according to claim 1, characterized in that: After the temperature of the enamel reactor is raised to 60° C., the reactor is kept warm for 3 to 5 hours until the total content of R1ONa, R1OH, R1COOR2 and R1COCl in the reactor is ≤0.1%. The step of stopping the aging includes: Detect the total content of R1ONa, R1OH, R1COOR2 and R1COCl in the enameled reactor.