Precursor beta-ketimino ethylene glycol dimethyl ether Fe (II) compound for magnetic random storage material
By using β-ketoimidoethylene glycol dimethyl ether Fe(II) compound as the Fe precursor, the existing Fe precursor has solved the problem of low water oxygen resistance and insufficient types, and achieved a low-cost, high-purity FeOx film The preparation of magnetic random storage materials simplifies the preparation process.
Patent Information
- Application Number
- CN202411181399.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN119080846A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a precursor beta-ketoimino glycol dimethyl ether Fe(II) compound for magnetic random storage material, belonging to the technical field of microelectronic materials. Background Art
[0002] With the development of the Internet, the Internet of Things and big data, information storage technology is constantly facing new requirements and challenges. The core of the development of information storage technology lies in information storage materials, and major countries and companies around the world have invested huge research and development efforts in this regard. Among them, magnetic random access storage technology uses a device with a large magnetoresistance effect to store data in a stable magnetic state. The data is read out by measuring the resistance of the device. Compared with other random access storage technologies, it has obvious advantages such as high integration, high-speed reading and writing capabilities, nearly infinite repeated read and write times, low power consumption and high radiation resistance, and the most outstanding non-volatility. The key to the development of magnetic random access storage technology lies in the development of magnetic random access storage materials. The current magnetic random access storage materials are mainly composed of appropriate ferromagnetic materials and their alloys, mainly including Fe-based metals Fe, CoFe, NiFe, CoFeB, FeO x And other metal or metal alloy thin film materials.
[0003] Traditional preparation methods of magnetic random access memory materials mainly include magnetron sputtering, molecular beam epitaxy, pulsed laser deposition and other methods. However, with the continuous reduction of the characteristic size of microelectronic devices and the continuous increase of the aspect ratio of the device structure, material filling faces great difficulties. The traditional deposition method can no longer meet the requirements (the method deposits materials faster at the opening of the groove, but slower at the bottom of the groove, which will lead to poor step coverage at the bottom of the groove and cause device failure). Chemical vapor deposition (CVD) and atomic layer deposition (ALD) technology have become new device manufacturing technologies due to their advantages in good conformality and uniformity. In CVD / ALD process technology, the properties of the precursor are crucial. The precursor is required to have excellent volatility, thermal stability and reactivity. In addition, it is also required to have high purity, easy storage, non-toxicity, easy synthesis, low price and as high water and oxygen stability as possible, so as to facilitate operation, use, storage and transportation. Therefore, whether there is a suitable precursor affects the success or failure of the entire CVD / ALD process.
[0004] Most of the Fe precursors reported so far have low water and oxygen stability, which makes them inconvenient to prepare, synthesize, and operate. At the same time, different precursors will directly affect the composition and performance of the final thin film materials due to their own structure and process parameters. The types and quantities of Fe precursors developed so far are relatively small and are not enough to meet the huge demand for the preparation of materials of different types and performances. Therefore, in the context of continuous upgrading of related technical fields, it is very important to explore the synthesis of more types of CVD / ALD Fe precursors to meet the increasing / improved needs. Summary of the invention
[0005] In order to solve at least one of the above problems, the purpose of the present invention is to provide a new type of iron precursor β-ketoimino glycol dimethyl ether Fe(II) compound for magnetic random access memory material, which has a simple synthesis method and mild synthesis conditions, has good solubility in organic solvents such as n-hexane, toluene, ether, dichloromethane, tetrahydrofuran, etc., has good volatility, thermal stability and air moisture resistance, and has good film-forming properties.
[0006] The first object of the present invention is to provide a β-ketoimino glycol dimethyl ether Fe(II) compound having a structure shown in the general formula (I):
[0007]
[0008] Wherein, R is a hydrogen atom, a C1-C6 alkyl group, a C2-C5 alkenyl group, a C2-C5 cycloalkyl group, a C6-C 10 Aryl or -Si(R 1 )3, R 1 It is a C1-C6 alkyl group.
[0009] In one embodiment of the present invention, the structure of the β-ketoimino glycol dimethyl ether Fe(II) compound specifically includes:
[0010]
[0011] A second object of the present invention is to provide a method for preparing the above-mentioned β-ketoimino glycol dimethyl ether Fe (II) compound, the method specifically comprising the following steps:
[0012] (1) dissolving a β-ketimine compound in ether, adding sodium hydride under stirring at -78 to 0°C, then returning to room temperature and continuing to stir for 24 to 48 hours to obtain a reaction mixture;
[0013] (2) According to the molar ratio of β-ketimine or its derivatives to ferric chloride and ethylene glycol dimethyl ether: 2: (0.9-1.1):
[0014] (0.9-1.1), weigh a certain amount of ferric chloride and ethylene glycol dimethyl ether, dissolve them in ether to obtain a ferric chloride-ethylene glycol dimethyl ether ether solution;
[0015] (3) adding the reaction mixture obtained in step (1) to the ferric chloride-ethylene glycol dimethyl ether ether solution obtained in step (2) at -78°C, slowly heating to room temperature at a heating rate of 0.5 to 1°C / min, and continuing to stir and react at room temperature for 10 to 24 hours;
[0016] (4) After the reaction in step (3) is completed, the volatile matter is removed by decompression, and then a hexane or toluene solution is added to dissolve, filtered and extracted, the filtrate is collected, and the β-ketoimino glycol dimethyl ether Fe (II) compound is obtained after repeated recrystallization at -30°C.
[0017] In one embodiment of the present invention, in step (1), the mass ratio of the β-ketoimine compound to the diethyl ether is 1:10 to 1:20.
[0018] In one embodiment of the present invention, in step (1), the molar ratio of β-ketimine or its derivative to sodium hydride is 1:1 to 1:1.2.
[0019] In one embodiment of the present invention, the stirring speed in step (1) is 100 to 1000 rpm.
[0020] In one embodiment of the present invention, the mass ratio of ferric chloride to diethyl ether in step (2) is 1:10 to 1:20.
[0021] The third object of the present invention is to provide the application of the above-mentioned β-ketoimino glycol dimethyl ether Fe(II) compound in the field of microelectronic material preparation.
[0022] In one embodiment of the present invention, the application is for preparing magnetic random information storage materials.
[0023] In one embodiment of the present invention, the application is to use the above-mentioned β-ketoimino glycol dimethyl ether Fe(II) compound as a precursor to prepare a metal or metal alloy film through a chemical vapor deposition process or an atomic layer deposition process.
[0024] Beneficial effects of the present invention:
[0025] The β-ketoimino glycol dimethyl ether Fe(II) compound obtained by the present invention can be used as a precursor for CVD / ALD, and Fe-based thin films such as FeOx are prepared by chemical vapor deposition (CVD) or atomic layer deposition (ALD) processes. The β-ketoimino glycol dimethyl ether Fe(II) compound described in the present invention has the following advantages: (1) The synthesis method is simple and the conditions are mild, which greatly reduces the synthesis cost of the precursor material; (2) It has good solubility in organic solvents such as n-hexane, toluene, ether, dichloromethane, tetrahydrofuran, etc., making the transportation, delivery and processing of the precursor simple and easy to operate; (3) It has good air moisture resistance stability, making the operation, transportation, delivery and processing of the precursor simple and easy to operate; (4) It has good volatility and thermal stability. For example, after testing the thermal properties of the precursor by thermogravimetric (TG) method, the T of the dimethyl β-ketoimino glycol dimethyl ether Fe(II) precursor under normal pressure is 50 The minimum residual mass is 2.6% at 231.9℃; (5) It has good film-forming properties. Taking the dimethyl β-ketoimino glycol dimethyl ether Fe(II) precursor as an example, with N2 as the carrier gas and O2 as the reaction gas, a good CVD FeO can be formed at 500℃. X The film is uniform and continuous with high purity. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the single crystal structure diagram of the Fe(II) precursor of dimethyl β-ketoimino glycol dimethyl ether;
[0027] Figure 2 It is the TG spectrum of the dimethyl β-ketoimino glycol dimethyl ether Fe(II) precursor, the abscissa is the temperature, the unit is oC, the ordinate is the weight loss rate, the unit is %;
[0028] Figure 3 This is the SEM image of the CVD thin film material obtained using the dimethyl β-ketoimino glycol dimethyl ether Fe(II) precursor;
[0029] Figure 4 This is the XPS graph of the CVD thin film material obtained using dimethyl β-ketoimino glycol dimethyl ether Fe(II) precursor. DETAILED DESCRIPTION
[0030] In order to more clearly understand the technical content of the present invention, the following examples are given in detail, the purpose of which is only to better understand the content of the present invention but not to limit the protection scope of the present invention.
[0031] The preparation method of the β-ketoimino glycol dimethyl ether Fe(II) precursor of the present invention is carried out according to the following reaction route:
[0032]
[0033] Example 1
[0034] A method for preparing a precursor β-ketoimino glycol dimethyl ether Fe(II) compound for magnetic random access memory material comprises the following steps:
[0035] (1) dissolving methyl β-ketimine in ether, wherein the mass ratio of methyl β-ketimine to ether solvent is 1:20, adding sodium hydride under stirring at -78°C, wherein the molar ratio of methyl β-ketimine to sodium hydride is 1:1, and the stirring speed is 700 rpm; after returning to room temperature, stirring and reacting for 24 hours to obtain a reaction mixture;
[0036] (2) weighing a certain amount of ferric chloride and ethylene glycol dimethyl ether in a molar ratio of 2:1:1 of methyl β-ketoimine to ferric chloride and ethylene glycol dimethyl ether, dissolving them in ether to obtain a ferric chloride-ethylene glycol dimethyl ether ether solution; wherein the mass ratio of ferric chloride to ether is 1:20;
[0037] (3) adding the reaction mixture obtained in step (1) to the ferric chloride-ethylene glycol dimethyl ether ether solution obtained in step (2) at -78°C, slowly heating to room temperature at a heating rate of 1°C / min, and continuing to stir and react at room temperature for 15 hours;
[0038] (4) After the reaction in step (3) is completed, the volatile matter is removed by reducing pressure, and then a hexane solution is added to dissolve, filtered and extracted, the filtrate is collected, and the target product is obtained after repeated recrystallization at -30°C.
[0039] The structural formula of the target product is: Yield: 65%, elemental analysis: C, 51.98; H, 8.53; N, 7.76, Fe, 14.90; theoretical elemental analysis values are C, 51.62; H, 8.66; N, 7.52; Fe, 15.00. The structure of the target product was analyzed by single crystal X-ray diffraction, and the specific structural formula is as follows Figure 1 shown.
[0040] The synthesized dimethyl β-ketoimino glycol dimethyl ether iron precursor has good solubility in organic solvents such as n-hexane, toluene, ether, dichloromethane, tetrahydrofuran, etc., and the synthesized precursor has good air moisture stability and can be stored in the atmospheric environment for more than 2 days without deterioration, making the transportation, delivery and processing of the precursor simple and easy to operate;
[0041] The thermal properties of the precursor were tested by thermogravimetric (TG) method. The T 50is 231.9℃, the minimum residual mass is 2.6%, the results are shown in Figure 2 , has good volatility and thermal stability.
[0042] CVD deposited thin films:
[0043] The target product was used as a precursor. The growth parameters used in the CVD deposition process were: total pressure 10 torr, N2 flow rate: 120 mL / min, O2 flow rate: 100 mL / min, deposition time: 20 min, deposition temperature: 500 °C, film formation rate: 5.1 nm / min. The SEM and XPS images of the deposited film are shown in Figure 3 and Figure 4 , the film formation is continuous and uniform with high purity.
[0044] Example 2
[0045] A method for preparing a precursor β-ketoimino glycol dimethyl ether Fe(II) compound for magnetic random access memory material comprises the following steps:
[0046] (1) dissolving phenyl β-ketimine in ether, wherein the mass ratio of methyl β-ketimine to ether solvent is 1:25, adding metallic lithium under stirring at -78°C, wherein the molar ratio of phenyl β-ketimine to sodium hydride is 1:1.2, and the stirring speed is 800 rpm; after returning to room temperature, stirring and reacting for 48 hours, a reaction mixture is obtained;
[0047] (2) weighing a certain amount of ferric chloride and ethylene glycol dimethyl ether in a molar ratio of phenyl β-ketimine to ferric chloride and ethylene glycol dimethyl ether of 2:1:1, dissolving them in diethyl ether to obtain a ferric chloride-ethylene glycol dimethyl ether solution; wherein the mass ratio of ferric chloride to diethyl ether is 1:25;
[0048] (3) adding the reaction mixture obtained in step (1) to the ferric chloride-ethylene glycol dimethyl ether ether solution obtained in step (2) at -78°C, slowly heating to room temperature at a heating rate of 0.5°C / min, and continuing to stir and react at room temperature for 15 hours;
[0049] (4) After the reaction in step (3) is completed, the volatile matter is removed by reducing pressure, and then a hexane solution is added to dissolve, filtered and extracted, the filtrate is collected, and the target product is obtained after repeated recrystallization at -30°C.
[0050] The structural formula of the target product is: Yield: 57%, elemental analysis: C, 62.73; H, 7.41; N, 5.77, Fe, 11.16; theoretical elemental analysis values are C, 62.91; H, 7.31; N, 5.64, Fe, 11.25.
[0051] The synthesized bisphenyl β-ketoimino glycol dimethyl ether iron precursor has good solubility in organic solvents such as n-hexane, toluene, ether, dichloromethane, tetrahydrofuran, etc., and the synthesized precursor has good air moisture stability and can be stored in the atmospheric environment for more than 2 days without deterioration, making the transportation, delivery and processing of the precursor simple and easy to operate;
[0052] The thermal properties of the precursor were tested by thermogravimetric (TG) method. The T 50 The temperature is 256.1℃, the minimum residual mass is 6.4%, and it has good volatility and thermal stability.
[0053] CVD deposited thin films:
[0054] The target product was used as a precursor, and the growth parameters used in the CVD deposition process were: total pressure 10 torr, N2 flow rate: 120 mL / min, O2 flow rate: 100 mL / min, deposition time: 20 min, deposition temperature: 500°C, and film formation rate: 4.3 nm / min.
[0055] Example 3
[0056] A method for preparing a precursor β-ketoimino glycol dimethyl ether Fe(II) compound for magnetic random access memory material comprises the following steps:
[0057] (1) dissolving trimethylsilyl β-ketoimine in ether, wherein the mass ratio of trimethylsilyl β-ketoimine to ether solvent is 1:15, adding sodium hydride under stirring at -78°C, wherein the molar ratio of trimethylsilyl β-ketoimine to sodium hydride is 1:1.1, and the stirring speed is 600 rpm; after returning to room temperature, stirring and reacting for 30 hours to obtain a reaction mixture;
[0058] (2) weighing a certain amount of ferric chloride and ethylene glycol dimethyl ether in a molar ratio of trimethylsilyl β-ketoimine to ferric chloride and ethylene glycol dimethyl ether of 2:1:1, dissolving them in diethyl ether to obtain a ferric chloride-ethylene glycol dimethyl ether solution; wherein the mass ratio of ferric chloride to diethyl ether is 1:15;
[0059] (3) adding the reaction mixture obtained in step (1) to the ferric chloride-ethylene glycol dimethyl ether ether solution obtained in step (2) at -78°C, slowly heating to room temperature at a heating rate of 0.5°C / min, and continuing to stir and react at room temperature for 20 hours;
[0060] (4) After the reaction in step (3) is completed, the volatile matter is removed by reducing pressure, and then a hexane solution is added to dissolve, filtered and extracted, the filtrate is collected, and the target product is obtained after repeated recrystallization at -30°C.
[0061] The structural formula of the target product is: Yield: 61%, elemental analysis: C, 49.31; H, 9.17; N, 5.65, Fe, 11.23; theoretical elemental analysis values are C, 49.17; H, 9.08; N, 5.73; Fe, 11.43.
[0062] The synthesized bistrimethylsilyl β-ketoimino glycol dimethyl ether iron precursor has good solubility in organic solvents such as n-hexane, toluene, ether, dichloromethane, tetrahydrofuran, etc., and the synthesized precursor has good air moisture stability and can be stored in the atmospheric environment for more than 2 days without deterioration, making the transportation, delivery and processing of the precursor simple and easy to operate;
[0063] The thermal properties of the precursor were tested by thermogravimetric (TG) method. The T 50 The temperature is 243.8℃, the minimum residual mass is 5.1%, and it has good volatility and thermal stability.
[0064] CVD deposited thin films:
[0065] The target product was used as a precursor, and the growth parameters used in the CVD deposition process were: total pressure 10 torr, N2 flow rate: 120 mL / min, O2 flow rate: 100 mL / min, deposition time: 20 min, deposition temperature: 500°C, and film formation rate: 3.6 nm / min.
[0066] Comparative Example 1
[0067] The Fe complex containing O-type ligands, ferrous acetylacetonate, was used as a precursor for CVD / ALD thin film deposition, and its properties were compared with those of the precursor in Example 1. The structure of the ferrous acetylacetonate complex is as follows:
[0068]
[0069] The precursor has poor stability against water and oxygen and is easily hydrolyzed and deteriorated when encountering water and oxygen. In addition, the precursor has poor volatility and thermal stability, which increases the difficulty of the operation, transportation, delivery and processing of the precursor.
[0070] Comparative Example 2
[0071] The Fe complex containing N-type ligands, guanidine Fe, was used as a precursor for CVD / ALD thin film deposition, and its properties were compared with those of the precursor in Example 1. The structure of the guanidine Fe complex is as follows:
[0072]
[0073] The precursor has poor stability against water and oxygen and is prone to hydrolysis and deterioration when exposed to water and oxygen, which increases the difficulty of the operation, transportation, delivery and processing of the precursor and is not conducive to industrial application.
[0074] Comparative Example 3
[0075] The ferrocene complex was used as a precursor for CVD / ALD thin film deposition, and its properties were compared with those of the precursor in Example 1. The structure of the ferrocene complex is as follows:
[0076]
[0077] Although the precursor has high water and oxygen resistance stability, high volatility and thermal stability, the film prepared by the precursor tends to have a high impurity content, which is not conducive to industrial application.
[0078] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A β-ketoimino glycol dimethyl ether Fe(II) compound having a structure represented by the general formula (I): in, R is a hydrogen atom, a C1-C6 alkyl group, a C2-C5 alkenyl group, a C2-C5 cycloalkyl group, a C6-C 10 Aryl or -Si(R 1 )3.
2. The β-ketoimino glycol dimethyl ether Fe(II) compound according to claim 1, characterized in that Its structure includes:
3. The method for preparing the β-ketoimino glycol dimethyl ether Fe(II) compound according to claim 1, characterized in that: The method comprises the following steps: (1) dissolving a β-ketimine compound in ether, adding sodium hydride under stirring at -78 to 0°C, then returning to room temperature and continuing to stir for 24 to 48 hours to obtain a reaction mixture; (2) According to the molar ratio of β-ketimine or its derivatives to ferric chloride and ethylene glycol dimethyl ether: 2: (0.9-1.1): (0.9-1.1), weigh a certain amount of ferric chloride and ethylene glycol dimethyl ether, dissolve them in ether to obtain a ferric chloride-ethylene glycol dimethyl ether ether solution; (3) adding the reaction mixture obtained in step (1) to the ferric chloride-ethylene glycol dimethyl ether ether solution obtained in step (2) at -78°C, slowly heating to room temperature at a heating rate of 0.5 to 1°C / min, and continuing to stir and react at room temperature for 10 to 24 hours; (4) After the reaction in step (3) is completed, the volatile matter is removed by decompression, and then a hexane or toluene solution is added to dissolve, filtered and extracted, the filtrate is collected, and the β-ketoimino glycol dimethyl ether Fe (II) compound is obtained after repeated recrystallization at -30°C.
4. The method according to claim 3, characterized in that In step (1), the mass ratio of the β-ketimine compound to the ether is 1:10 to 1:
20.
5. The method according to claim 3, characterized in that: In step (1), the molar ratio of β-ketimine or its derivative to sodium hydride is 1:1 to 1:1.
2.
6. The method according to any one of claims 3 to 5, characterized in that: In step (2), the mass ratio of ferric chloride to ether is 1:10 to 1:
20.
7. Use of the β-ketoimino glycol dimethyl ether Fe(II) compound according to claim 1 or 2 in the field of preparation of magnetic random access memory materials.
8. The use according to claim 7, characterized in that: The application is to use the β-ketoimino glycol dimethyl ether Fe (II) compound described in claim 1 or 2 as a precursor to prepare a metal or metal alloy film through a chemical vapor deposition process or an atomic layer deposition process.