Ionic aromatic framework material with rapid high-humidity detection performance and preparation method of ionic aromatic framework material

The ionic aromatic frame material PAF1'-I synthesized through Yamamoto-type Ullmann coupling reaction solves the problem of unstable existing humidity sensing materials in high humidity and corrosive environments, and achieves high specific surface area and continuous open channels, which significantly It improves the adsorption capacity and response speed of water molecules, and is suitable for humidity monitoring in harsh environments.

CN119081145AActive Publication Date: 2024-12-06XI AN JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411265108.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Existing humidity sensing materials show instability in high humidity and corrosive environments. Ceramic materials absorb and desorb water molecules for a long time and have few active sites, while polymer materials are susceptible to damage in low humidity environments. It is difficult to achieve fast and reliable humidity monitoring.

Method used

Using the Yamamoto Ullmann coupling reaction principle, the ionic aromatic frame material PAF1'-I with phosphate structure regulation ability is synthesized through hydrogen bonding of phosphate groups and the avidity of water molecules of metal cations to ensure the high specific surface area of ​​the material. and continuously open humidity transmission channels to improve the adsorption capacity and response speed of water molecules.

Benefits of technology

It has achieved significantly improved water molecules adsorption capacity and response speed in humidity sensing. The material has strong selective adsorption ability to water molecules and can maintain good humidity sensing performance within the range of 11%-95% RH, which is suitable for strict Humidity monitoring in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005036903520000021
    Figure BDA0005036903520000021
  • Figure BDA0005036903520000051
    Figure BDA0005036903520000051
  • Figure FDA0005036903510000011
    Figure FDA0005036903510000011
Patent Text Reader

Abstract

The invention provides an ionic aromatic framework material with rapid and reliable humidity detection performance and a preparation method thereof, and according to a Yamamoto-type Ullmann coupling reaction principle, the ionic aromatic framework material with rapid and reliable humidity detection performance is finally obtained by utilizing a substitution reaction of aryl and a chlorophosphate group and a neutralization reaction of a phosphate group and hydroxide. According to the invention, a permanently open humidity transmission channel and a high specific surface area of the adsorbent are ensured, the material can be ensured to improve the adsorption capacity of water molecules through structural adjustment, and the material is expected to show remarkable advantages in humidity sensing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of ionic porous aromatic skeleton materials, and in particular relates to an ionic aromatic framework material with rapid high-humidity detection performance and a preparation method thereof. Background Art

[0002] As a component of humidity sensors, the physical and chemical properties of sensing materials directly affect the performance of sensors. Currently, there are two main types of sensing materials that can be applied in practice: ceramics and polymer materials. Commercial ceramic sensing materials have good physical and chemical stability, but the absorption and desorption of water molecules takes a long time, especially the desorption process often requires heating to expel water molecules; another disadvantage is that ceramic materials have few active sites, and it is difficult to maintain a good working condition in the entire humidity range, and it is impossible to capture and respond to signals when the humidity is low. Polymer materials are a type of sensing material that can be detected in low humidity areas by introducing a large number of active groups into the organic chain, but their stability and anti-interference ability are far inferior to ceramic materials. In corrosive or flue gas environments, the structure is easily damaged, resulting in errors and failures. Therefore, the development of fast and reliable sensing materials is of great significance for humidity monitoring in harsh environments.

[0003] In humidity sensing, the performance of humidity sensors is determined by the selective adsorption of water molecules by the sensing material and the construction of ion transport channels. At present, porous sensing materials such as zeolite molecular sieves and metal organic framework materials (MOFs) are used in humidity sensing research. Zeolite molecular sieves have the advantages of low cost, easy preparation, and large specific surface area, but the amount of water adsorbed by a small amount of hydroxyl groups in the pores is limited, and the humidity monitoring range is greatly restricted. MOFs have also been widely used in sensing research in recent years and have shown excellent water molecule adsorption effects, but MOFs materials have poor acid and alkali resistance, high humidity resistance, and thermal stability. In the face of high humidity meteorological environments in rainy seasons and high temperature corrosive factory environments, their application range and reusability are subject to certain restrictions. Summary of the invention

[0004] The purpose of the present invention is to provide an ionic aromatic framework material (PAF1′-I) with rapid and high humidity detection performance and a preparation method thereof, so as to overcome the problems existing in the prior art. The present invention is based on the principle of Yamamoto-type Ullmann coupling reaction, and utilizes the hydrogen bonding effect of phosphate groups and the affinity of metal cations for water molecules. The synthesized PAF1′-I material has ion regulation ability and can achieve structural regulation of different phosphates. This not only ensures the permanent open humidity transmission channel and high specific surface area of ​​the adsorbent, but also ensures that the material can increase the adsorption capacity of water molecules through structural adjustment, which is expected to show significant advantages in humidity sensing.

[0005] The present invention is achieved through the following technical solutions:

[0006] An ionic aromatic framework material with fast and reliable humidity detection performance, the structural formula of which is shown below:

[0007]

[0008] A method for preparing an ionic aromatic framework material with rapid and reliable humidity detection performance, based on the Yamamoto-type Ullmann coupling reaction principle, utilizing the substitution reaction of an aromatic group with a chlorophosphate group, and the neutralization reaction of a phosphate group with a hydroxide, to finally obtain an ionic aromatic framework material with rapid and reliable humidity detection performance;

[0009] The specific steps include:

[0010] Step 1: Under a nitrogen atmosphere, nickel nitrate, 2,2'-bipyridine, zinc powder, and tetrakis(4-bromophenyl)methane are added to a solvent, and heated and stirred for reaction; after the reaction is completed, the mixture is cooled to room temperature, water is added to the reaction mixture, the precipitated solid product is collected by filtration, and washed with water, ethanol, and tetrahydrofuran several times in sequence to obtain a white solid PAF1;

[0011] Step 2: In an inert atmosphere, white solid PAF1 was mixed with chlorophosphoric acid in DMF, stirred at room temperature, then washed with water several times, and finally vacuum dried to obtain PAF1′ modified with a phosphate group;

[0012] Step 3: Mix the PAF1′ modified with a phosphate group obtained in step 2 and a hydroxide base in a preset ratio and add them to a methanol solution, stir thoroughly, wash repeatedly with water and methanol respectively, and finally vacuum dry to obtain the ionic porous aromatic framework material PAF1′-I.

[0013] Furthermore, in step 1, the ratio of nickel nitrate, 2,2'-bipyridine, zinc powder, tetrakis(4-bromophenyl)methane and solvent is 2.105mmol:2.105mmol:10.0mmol:0.3mmol:20mL.

[0014] Furthermore, in step 1, the temperature of the heating and stirring reaction is 40° C. and the time is 60 h.

[0015] Furthermore, the solvent in step 1 is N,N-dimethylformamide.

[0016] Furthermore, in step 2, the mass ratio of white solid PAF1 to chlorophosphoric acid is 1:1.53.

[0017] Furthermore, in step 2, the stirring time is 30 hours, and the vacuum drying temperature is 120°C.

[0018] Furthermore, in step 3, the hydroxide base is sodium hydroxide, potassium hydroxide or magnesium hydroxide;

[0019] The mass volume ratio of the PAF1′ modified with a phosphate group, the hydroxide base and methanol is 0.062 g:0.062 g:30 mL.

[0020] Furthermore, the stirring time in step three is 20 hours.

[0021] Furthermore, in step three, the vacuum drying temperature is 110° C. and the time is 12 h.

[0022] Compared with the prior art, the present invention has the following beneficial technical effects:

[0023] The ionic porous aromatic framework material (PAF1′-I) of the present invention has a high specific surface area and phosphate structure adjustment capability, and can dissociate and transmit ions under humidity stimulation. In theory, the empty framework structure constructed by the porous material is not conducive to the formation of a continuous ion transmission channel, and the introduction of phosphates on the framework can shorten the distance between the adsorbed water molecules, which not only ensures that the material can increase the adsorption capacity of water molecules through structural adjustment, but also ensures that the adsorbent has a continuous and open transmission channel. However, the water molecules adsorbed by the framework of most materials are always widely spaced, resulting in interruptions in the transmission channel, making it difficult for ions to jump and transfer to form ionic conductivity, thereby affecting the transmission speed, which is manifested in the sensor as a slower response speed.

[0024] The aromatic conjugated units of the material have obvious advantages in providing a controllable and stable transmission channel. The pore size of the PAF1′ material is mainly distributed in the range of 0.82-1.47 nm, which provides sufficient space for ion transmission. The PAF1′-I material obtained by the present invention has good selective adsorption capacity for water molecules. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. The following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 The XRD pattern of the PAF1′-I material prepared in Example 1-3;

[0027] Figure 2The scanning electron microscope images of the PAF1′-I materials prepared in Examples 1-3, wherein (a) is a scanning electron microscope image of PAF1′-Na, (b) is a scanning electron microscope image of PAF1′-K, and (c) is a scanning electron microscope image of PAF1′-Mg;

[0028] Figure 3 The EDS graphs of the PAF1′-I materials prepared in Examples 1-3, wherein (a) is the EDS graph of PAF1′-Na, (b) is the EDS graph of PAF1′-K, and (c) is the EDS graph of PAF1′-Mg;

[0029] Figure 4 The impedance-frequency humidity sensing graph of the PAF1′-I material prepared in Example 1-3;

[0030] Figure 5 The response-recovery time diagrams of the PAF1′-I materials prepared in Examples 1-3, wherein (a) is the response-recovery time diagram of PAF1′-Na, (b) is the response-recovery time diagram of PAF1′-K, and (c) is the response-recovery time diagram of PAF1′-Mg;

[0031] Figure 6 These are the hysteresis diagrams of the PAF1′-I materials prepared in Examples 1-3, wherein (a) is the hysteresis diagram of PAF1′-Na, (b) is the hysteresis diagram of PAF1′-K, and (c) is the hysteresis diagram of PAF1′-Mg. DETAILED DESCRIPTION

[0032] The present invention is described in detail below:

[0033] The present invention provides an ionic aromatic framework material with rapid and reliable humidity detection performance, the structural formula of which is shown in formula (I):

[0034]

[0035] The steps include:

[0036] Step 1: Under a nitrogen atmosphere, add 2.105 mmol nickel nitrate, 2.105 mmol 2,2'-bipyridine, 10.0 mmol zinc powder, and 0.3 mmol tetrakis(4-bromophenyl)methane to 20 mL N,N-dimethylformamide (DMF), and stir at 40°C for 60 hours; after the reaction is completed, cool to room temperature, add water to the reaction mixture, collect the precipitated solid product by filtration, and wash it several times with water, ethanol, and tetrahydrofuran to obtain a white solid PAF1.

[0037] Step 2: In an inert atmosphere, white solid PAF1 and chlorophosphoric acid (mass ratio of 1:1.53) were mixed in DMF, stirred at room temperature for 30 hours, washed with water several times, and dried under vacuum at 120°C to obtain PAF1′ modified with a phosphate group.

[0038] Step 3: PAF1′ modified with a phosphate group obtained in step 2 and a hydroxide base (sodium hydroxide, potassium hydroxide or magnesium hydroxide) were mixed and added to a methanol solution (the mass volume ratio of PAF1′ modified with a phosphate group, the hydroxide base and methanol was 0.062 g:0.062 g:30 mL), and stirred for 20 h. 2 The reaction mixture was repeatedly washed with O and methanol and dried in vacuo at 110 °C to obtain an ionic porous aromatic framework material (PAF1′-I, where I represents Na / K / Mg).

[0039] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.

[0040] The following detailed description is the description of the embodiments, and is intended to provide further detailed description of the present invention. Unless otherwise specified, all technical terms used in the present invention have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used in the present invention are only for describing specific embodiments, and are not intended to limit the exemplary embodiments according to the present invention.

[0041] Example 1

[0042] Step 1: Under a nitrogen atmosphere, add 2.105 mmol nickel nitrate, 2.105 mmol 2,2'-bipyridine, 10.0 mmol zinc powder, and 0.3 mmol tetrakis(4-bromophenyl)methane to 20 mL N,N-dimethylformamide and stir at 40°C for 60 hours; after the reaction is completed, cool to room temperature, add water to the reaction mixture, collect the precipitated solid product by filtration, and wash it several times with water, ethanol, and tetrahydrofuran to obtain a white solid PAF1.

[0043] Step 2: In an inert atmosphere, 1 mg of PAF1 was mixed with 1.53 mg of chlorophosphoric acid in DMF, stirred at room temperature for 30 h, washed with water several times, and dried under vacuum at 120 °C to obtain PAF1′ modified with a phosphate group.

[0044] Step 3: 0.062 g of the product PAF1′ obtained in step 2 and 0.062 g of sodium hydroxide were mixed and added into 30 mL of methanol solution, stirred for 20 h, and then 2 The reaction mixture was washed repeatedly with O and methanol and dried under vacuum at 110 °C to obtain an ionic porous aromatic framework material (PAF1′-Na).

[0045] Example 2

[0046] Step 1: Under a nitrogen atmosphere, add 2.105 mmol nickel nitrate, 2.105 mmol 2,2'-bipyridine, 10.0 mmol zinc powder, and 0.3 mmol tetrakis(4-bromophenyl)methane to 20 mL N,N-dimethylformamide and stir at 40°C for 60 hours; after the reaction is completed, cool to room temperature, add water to the reaction mixture, collect the precipitated solid product by filtration, and wash it several times with water, ethanol, and tetrahydrofuran to obtain a white solid PAF1.

[0047] Step 2: In an inert atmosphere, 1 mg of PAF1 was mixed with 1.53 mg of chlorophosphoric acid in DMF, stirred at room temperature for 30 h, washed with water several times, and dried under vacuum at 120 °C to obtain PAF1′ modified with a phosphate group.

[0048] Step 3: 0.062 g of the product PAF1′ obtained in step 2 and 0.062 g of potassium hydroxide were mixed and added into 30 mL of methanol solution, stirred for 20 h, and then 2 The reaction mixture was washed repeatedly with O and methanol and dried under vacuum at 110 °C to obtain an ionic porous aromatic framework material (PAF1′-K).

[0049] Example 3

[0050] Step 1: Under a nitrogen atmosphere, add 2.105 mmol nickel nitrate, 2.105 mmol 2,2'-bipyridine, 10.0 mmol zinc powder, and 0.3 mmol tetrakis(4-bromophenyl)methane to 20 mL N,N-dimethylformamide and stir at 40°C for 60 hours; after the reaction is completed, cool to room temperature, add water to the reaction mixture, collect the precipitated solid product by filtration, and wash it several times with water, ethanol, and tetrahydrofuran to obtain a white solid PAF1.

[0051] Step 2: In an inert atmosphere, 1 mg of PAF1 was mixed with 1.53 mg of chlorophosphoric acid in DMF, stirred at room temperature for 30 h, washed with water several times, and dried under vacuum at 120 °C to obtain PAF1′ modified with a phosphate group.

[0052] Step 3: 0.062 g of the product PAF1′ obtained in step 2 and 0.062 g of magnesium hydroxide were mixed and added into 30 mL of methanol solution, stirred for 20 h, and then treated with H 2 The obtained product was washed repeatedly with O and methanol and dried in vacuo at 110 °C to obtain an ionic porous aromatic framework material (PAF1′-Mg).

[0053] Figure 1These are the XRD spectra of PAF1′-Na, PAF1′-K and PAF1′-Mg materials prepared in Examples 1-3. It can be seen from the figures that the materials are amorphous.

[0054] Figure 2 These are the scanning electron micrographs of PAF1′-Na, PAF1′-K and PAF1′-Mg materials prepared in Examples 1-3. It can be seen from the figures that the introduction of ions has little effect on the morphology of PAF1′.

[0055] Figure 3 These are the EDS images of PAF1′-Na, PAF1′-K and PAF1′-Mg materials prepared in Examples 1-3. It can be seen from the images that the ions are evenly distributed in the materials.

[0056] Figure 4 The humidity-impedance diagrams of PAF1′-Na, PAF1′-K and PAF1′-Mg prepared in Examples 1-3 show that the sensitivity of PAF1′-Na is better than that of PAF1′-K and PAF1′-Mg, which may be due to the fact that the radius and affinity for water of Na are better than those of K and Mg.

[0057] Figure 5 This is the response recovery time diagram of PAF1′-Na, PAF1′-K, and PAF1′-Mg prepared in Example 1-3. The response recovery rate of PAF1′-Na is 12 / 24s, the response recovery rate of PAF1′-K is 18 / 39s, and the response recovery rate of PAF1′-Mg is 18 / 30s.

[0058] Figure 6 These are the hysteresis diagrams of PPAF1′-Na, PAF1′-K, and PAF1′-Mg prepared in Examples 1-3. The hysteresis differences of PAF1′-Na, PAF1′-K, and PAF1′-Mg are all less than 5% RH.

[0059] From the humidity sensing performance diagram of PAF1′-I material, it can be seen that PAF1′-Na, PAF1′-K, and PAF1′-Mg all exhibit good water molecule sensing performance. The humidity sensing range at room temperature can reach 11%-95% RH, which is much higher than the sensing performance of zeolite.

[0060] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. An ionic aromatic framework material with fast and reliable humidity detection performance, It is characterized in that Its structural formula is shown below:

2. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance as claimed in claim 1, It is characterized in that Based on the Yamamoto-type Ullmann coupling reaction principle, the substitution reaction between aromatic groups and chlorophosphate groups and the neutralization reaction between phosphate groups and hydroxides are used to finally obtain an ionic aromatic framework material with fast and reliable humidity detection performance. The specific steps include: Step 1: Under a nitrogen atmosphere, nickel nitrate, 2,2'-bipyridine, zinc powder, and tetrakis(4-bromophenyl)methane are added to a solvent, and heated and stirred for reaction; after the reaction is completed, the mixture is cooled to room temperature, water is added to the reaction mixture, the precipitated solid product is collected by filtration, and washed with water, ethanol, and tetrahydrofuran several times in sequence to obtain a white solid PAF1; Step 2: In an inert atmosphere, white solid PAF1 was mixed with chlorophosphoric acid in DMF, stirred at room temperature, then washed with water several times, and finally vacuum dried to obtain PAF1′ modified with a phosphate group; Step 3: Mix the PAF1′ modified with a phosphate group obtained in step 2 and a hydroxide base in a preset ratio and add them to a methanol solution, stir thoroughly, wash repeatedly with water and methanol respectively, and finally vacuum dry to obtain the ionic porous aromatic framework material PAF1′-I.

3. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance according to claim 2, It is characterized in that The ratio of nickel nitrate, 2,2'-bipyridine, zinc powder, tetrakis(4-bromophenyl)methane and solvent in step 1 is 2.105 mmol:2.105 mmol:10.0 mmol:0.3 mmol:20 mL.

4. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance according to claim 2, It is characterized in that The temperature of the heating and stirring reaction in step 1 is 40° C. and the time is 60 h.

5. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance according to claim 2, It is characterized in that The solvent in step 1 is N,N-dimethylformamide.

6. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance according to claim 2, It is characterized in that In step 2, the mass ratio of white solid PAF1 to chlorophosphoric acid is 1:1.

53.

7. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance according to claim 2, It is characterized in that In step 2, the stirring time is 30 h and the vacuum drying temperature is 120° C.

8. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance according to claim 2, It is characterized in that In step 3, the hydroxide base is sodium hydroxide, potassium hydroxide or magnesium hydroxide; The mass volume ratio of the PAF1′ modified with a phosphate group, the hydroxide base and methanol is 0.062 g:0.062 g:30 mL.

9. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance according to claim 2, It is characterized in that The stirring time in step 3 is 20h.

10. A method for preparing an ionic aromatic framework material having fast and reliable humidity detection performance according to claim 2, It is characterized in that The vacuum drying temperature in step 3 is 110° C. and the time is 12 h.

Citation Information

Patent Citations

  • Modified humidity-sensitive material, preparation method and application thereof, and humidity sensor

    CN114644888A

  • Electrical resistance humidity sensor comprised of an organic polymer

    KR1020010008930A