Anti-splashing film for glass and preparation method of anti-splashing film
Through the combination of cross-linking of polyurethane resin and cross-linking agent and functional particles of acrylic resin, the problem of anti-splash film for glass is solved, and more stable connection and higher hardness are achieved, and the anti-splash film is improved. Durability and scratch resistance.
Patent Information
- Application Number
- CN202411247679.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
AI Technical Summary
The existing anti-splash film for glass is prone to fall off after a long time of use, and is easily damaged when hit by flying sand during high-speed driving, making it difficult to effectively prevent glass from cracking and scratching.
Polyurethane resin is used as the crosslinking agent for the bridge layer to form a stable connection, and acrylic resin and functional particles are added to the hardening layer to enhance hardness and scratch resistance.
It effectively avoids the fall off and scratch damage of the anti-splash film, enhances the durability and scratch resistance of the anti-splash film for glass, and prevents damage caused by high-frequency and high-speed impact of fine particles during high-speed driving.
Smart Images

Figure CN119081202A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-splash films, and in particular relates to an anti-splash film for glass and a preparation method thereof. Background Art
[0002] Glass products are widely used in the transportation field, such as automotive glass, high-speed rail glass, etc. How to prevent the glass from being broken by external impact and causing glass slag to splash during high-speed driving has become a technical issue worthy of attention. In order to solve this technical problem, the traditional approach is to cover the surface of the glass with an anti-splash film, and bond the glass and the anti-splash film together with a PVB or EVA adhesive layer. When the glass is broken by external impact, the impact resistance of the anti-splash film prevents the glass from splashing. However, the structure of using a PVB adhesive layer to bond the glass and the anti-splash film for a long time has the risk of debonding, and the high-speed movement of vehicles often encounters flying sand impacts, and the kinetic energy of the impact is absorbed by the glass. The high-frequency and high-speed impact of fine particles can easily cause damage to the anti-splash film. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings and deficiencies in the prior art and provide an anti-splash film for glass. The polyurethane resin in the bridging layer can be cross-linked with the main substrate layer and the adhesive layer on the glass, so that the main substrate layer and the adhesive layer are firmly connected, thereby preventing the anti-splash film for glass from falling off after long-term use. The hardening layer enhances the hardness of the anti-splash film for glass, avoiding scratches caused by contact with the mold during processing, and at the same time preventing the high-frequency and high-speed impact of fine particles from causing damage to the anti-splash film for glass.
[0004] The present invention is achieved through the following technical solutions:
[0005] A splash-proof film for glass comprises a main substrate layer, a bridging layer and a hardening layer; the bridging layer and the hardening layer are respectively arranged on two sides of the main substrate layer; the bridging layer comprises a polyurethane resin, a tackifying component and a crosslinking agent; the polyurethane comprises one or more of thermoplastic acrylic resin, thermosetting acrylic resin, hydroxy acrylic resin, oil-free polyester resin, fluorine-containing silicone resin and epoxy-modified acrylic resin; the tackifying component comprises one or more of high-carboxyl polyester, epoxy resin and silane coupling agent; the hardening layer comprises acrylic resin, a photoinitiator and functional particles.
[0006] In the anti-splash film for glass provided by the present invention, a bridging layer is arranged on one side of a main substrate layer, the main polyurethane resin is cross-linked under the action of a cross-linking agent so that the bridging layer has a certain hardness, and the viscosity-increasing component provides the viscosity of the bridging layer. When the anti-splash film for glass is rolled up, the anti-splash film for glass has internal pressure, because the polyurethane resin of the bridging layer is cross-linked to produce a certain hardness, and the viscosity-increasing component is limited to control the adhesion, so that the bridging layers will not adhere to each other, and the bridging layer will not be deformed to affect the appearance when stored for a long time and causing local pressure concentration; the polyurethane resin in the bridging layer can be cross-linked with the main substrate layer and the adhesive layer on the glass, so that the main substrate layer and the adhesive layer are firmly connected, and the anti-splash film for glass is prevented from falling off after long-term use; the hardening layer enhances the hardness and scratch resistance of the anti-splash film for glass, avoids scratches caused by contact with the abrasive tool during processing, and can also prevent the high-frequency and high-speed impact of fine particles from causing damage to the anti-splash film for glass.
[0007] Furthermore, the bridging layer comprises the following components in parts by weight: 90-100 parts by weight of polyurethane resin, 1-10 parts by weight of tackifying component, and 5-20 parts by weight of crosslinking agent; wherein the weight of the tackifying component is 1-3 parts, and the tackifying component is polyester; or, the weight of the tackifying component is 2-8 parts, and the tackifying component is a silane coupling agent.
[0008] Furthermore, the cross-linking agent includes one or more of isocyanate adducts, isocyanate trimers, and biuret adducts.
[0009] Furthermore, the thickness of the bridging layer is 1-2 μm, and the hardness is HB-H.
[0010] Furthermore, in the hardening layer, the acrylic resin includes at least one of UV epoxy acrylate, UV polyurethane acrylate, UV polyester acrylate, and UV pure acrylate.
[0011] Furthermore, the functional particles include at least one of breathable particles, heat-insulating particles and antibacterial particles; the breathable particles include at least one of inorganic glass and organic resin microspheres, with an average particle size of 0.1 μm; the heat-insulating particles include glass fiber reinforced plastic, with an average particle size of 1-1.5 μm; the antibacterial particles include nano zinc oxide, with an average particle size of 5-10 nm.
[0012] Furthermore, the hardening layer comprises the following components in parts by weight: 90-100 parts by weight of acrylic resin, 3-8 parts by weight of photoinitiator, and 0.3-1.5 parts by weight of functional particles.
[0013] Furthermore, the hardening layer has a thickness of 3-7 μm and a hardness of 2H-4H.
[0014] Furthermore, the main substrate layer includes at least one of PET, PE, and PP, the main substrate layer has a thickness of 100-200 μm, and the thickness ratio of the main substrate layer, the bridge layer, and the hardening layer is (10-20): (0.1-0.2): (0.3-0.7). An appropriate main substrate layer is selected to prevent the glass from splashing, a bridge layer of appropriate thickness connects the main substrate layer to the adhesive layer on the glass, and a hardening layer of appropriate thickness provides sufficient hardness to prevent scratches by external forces.
[0015] The present invention also provides a method for preparing the above-mentioned anti-splash film for glass, comprising the following steps:
[0016] The polyurethane resin, the tackifying component and the crosslinking agent are mixed according to the mass ratio, and then diluted with butyl acetate to a desired thickness of the bridging layer with a solid content of 10%, and stirred evenly until a transparent and uniform liquid phase is present to obtain a bridging layer solution;
[0017] The bridging layer solution is coated on the main substrate and dried to obtain a bridging layer on the main substrate, wherein the thickness of the bridging layer is 1-2 μm;
[0018] The acrylic resin, the photoinitiator and the functional particles are mixed according to a mass ratio and diluted with butyl acetate to a solid content of a required thickness of the hardening layer to obtain a hardening layer solution;
[0019] The hardening layer solution is applied to the side of the main substrate away from the bridging layer, dried, and then cured using a UV lamp;
[0020] The anti-splash film for glass is rolled up.
[0021] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the structure of an anti-splash film for glass.
[0023] Figure 2 It is a schematic diagram of the anti-splash film for glass being bonded to the glass.
[0024] Figure 3 It is a flow chart of preparing anti-splash film for glass. DETAILED DESCRIPTION
[0025] The embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the embodiments of the present invention, rather than to limit the embodiments of the present invention. It is also necessary to explain that, for ease of description, only parts related to the embodiments of the present invention are shown in the accompanying drawings, rather than all structures.
[0026] In addition, the terms first, second, third, etc. in the specification and claims are only used for the purpose of describing the same technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated, nor necessarily describing the order or time sequence. The terms are interchangeable where appropriate. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0027] Similarly, the terms "fixed" and "connected" used in the specification and claims should not be construed as limited to direct connection. Therefore, the expression "device A is connected to device B" should not be limited to a device or system in which device A is directly connected to device B, but means that there is a path between device A and device B, which may be a path including other devices or tools.
[0028] Example 1
[0029] This embodiment provides an anti-splash film for glass. Figure 1 The anti-splash film for glass comprises a main substrate layer 1, a bridge layer 2 and a hardening layer 3; the bridge layer 2 and the hardening layer 3 are respectively arranged on both sides of the main substrate layer 1;
[0030] The bridging layer 2 comprises a polyurethane resin, a tackifying component and a cross-linking agent;
[0031] In the bridging layer 2, the polyurethane resin includes one or more of thermoplastic acrylic resin, thermosetting acrylic resin, hydroxy acrylic resin, oil-free polyester resin, fluorine-containing silicone resin, and epoxy-modified acrylic resin; the viscosity-increasing component includes one or more of high-carboxyl polyester, epoxy resin, and silane coupling agent; the hardening layer 3 includes acrylic resin, photoinitiator, and functional particles.
[0032] In the anti-splash film for glass provided in this embodiment, the bridge layer 2 is arranged on one side of the main substrate layer 1, the polyurethane resin is cross-linked under the action of the cross-linking agent so that the bridge layer 2 has a certain hardness, and the viscosity-increasing component provides the viscosity of the bridge layer 2. When the anti-splash film for glass is rolled up, the anti-splash film for glass has internal pressure. Since the main polyurethane resin of the bridge layer 2 reacts with the cross-linking agent to produce a certain hardness and scratch resistance, and the viscosity-increasing component is limited to control the adhesion, the bridge layers 2 will not adhere to each other, and the bridge layer 2 will not be deformed and affect the appearance when the local pressure is concentrated due to long-term storage; the polyurethane resin in the bridge layer 2 can be cross-linked with the main substrate layer 1 and the adhesive layer 5 on the glass 4, so that the main substrate layer 1 and the adhesive layer 5 are firmly connected, and the anti-splash film for glass is prevented from falling off after long-term use; the hardening layer 3 enhances the hardness of the anti-splash film for glass, avoids scratches caused by contact with the construction mold 6 during processing, and can also prevent the high-frequency and high-speed impact of fine particles from damaging the anti-splash film for glass.
[0033] In this embodiment, the bridging layer comprises the following components in parts by weight: 90-100 parts by weight of polyurethane resin, 1-10 parts by weight of tackifying component, and 5-20 parts by weight of cross-linking agent;
[0034] Wherein, the weight portion of the tackifying component is 1-3 parts, and the tackifying component is polyester; or, the weight portion of the tackifying component is 2-10 parts, and the tackifying component is a silane coupling agent.
[0035] In this embodiment, the cross-linking agent of the bridging layer 2 includes one or more of isocyanate adducts, isocyanate trimers, and biuret adducts.
[0036] In this embodiment, the thickness of the bridging layer 2 is 1-2 μm, and the hardness is HB-H.
[0037] In this embodiment, the hardening layer includes the following components in parts by weight: 90-100 parts by weight of acrylic resin, 3-8 parts by weight of photoinitiator, and 0.3-1.5 parts by weight of functional particles.
[0038] In this embodiment, the acrylic resin in the hardening layer 3 includes at least one of UV epoxy acrylate, UV polyurethane acrylate, UV polyester acrylate, and UV pure acrylate.
[0039] In this embodiment, the photoinitiator of the hardening layer 3 includes at least one of a free radical initiator and a cationic photoinitiator. The free radical initiator includes at least one of 1173 free radical initiators, 184 free radical initiators, 907 free radical initiators, 369 free radical initiators, 1490 free radical initiators, and 1700 free radical initiators. The cationic initiator includes at least one of a diaryl iodonium salt, a triaryl iodonium salt, and an alkyl iodonium salt.
[0040] In this embodiment, the functional particles include at least one of breathable particles, heat-insulating particles and antibacterial particles; the breathable particles include at least one of inorganic glass and organic resin microspheres, with an average particle size of 0.1 μm; the heat-insulating particles include glass fiber reinforced plastic, with an average particle size of 1-1.5 μm; the antibacterial particles include nano zinc oxide, with an average particle size of 5-10 nm.
[0041] In this embodiment, the hardening layer 3 has a thickness of 3-7 μm and a hardness of 2H-4H.
[0042] In this embodiment, the main substrate layer 1 includes at least one of PET, PE, and PP, and has a thickness of 100-200 μm. The thickness ratio of the main substrate layer, the bridging layer, and the hardening layer is (10-20): (0.1-0.2): (0.3-0.7).
[0043] Example 2
[0044] This embodiment provides an anti-splash film for glass, comprising a main substrate layer 1, a bridging layer 2 and a hardening layer 3;
[0045] The main substrate layer 1 includes PET and has a thickness of 100 μm;
[0046] The bridging layer 2 includes polyurethane resin (PU2018 of Guangdong Keding New Materials Co., Ltd.), fluorine-containing silicone resin (AD7515W of Guangzhou Keding New Materials Co., Ltd.), biuret crosslinker (TDA-100 of Guangzhou Songwei Trading Co., Ltd.), and high-carboxyl polyester tackifier (CCK-208K of Huizhou Xiwo Trading Co., Ltd.), with a mass ratio of 50:50:15:1.5, a thickness of 1-2μm, and a hardness of HB. If the amount of biuret crosslinker added is too much, the bridging layer 2 will be too hard and unable to form a crosslink with the main substrate layer 1 to connect, thus losing the bridging effect; if the amount of biuret crosslinker added is too little, the bridging layer 2 will lack a certain physical strength, and the bridging layer 2 will be too soft, resulting in interlayer adhesion after the film is rolled up. If the amount of high-carboxyl polyester tackifier added is too large, the interlayer adhesion will occur after rolling up, while if the amount added is too small, the adhesion between the bridging layer 2 and the main substrate layer 1 will be reduced.
[0047] The hardening layer 3 includes UV polyurethane acrylate (6206C from Guangdong Lan Kelu New Materials Co., Ltd.), 184 photoinitiator particles (184 from Guangdong Lan Kelu New Materials Co., Ltd.) and thermal insulation particles, with a mass ratio of 100:5:0.5, a thickness of 6 μm and a hardness of 3H; the thermal insulation particles are glass fiber reinforced plastic particles (EMG11-20 from Shandong Dingshengxi Fiberglass Products Co., Ltd.).
[0048] Example 3
[0049] This embodiment provides an anti-splash film for glass, comprising a main substrate layer 1, a bridging layer 2 and a hardening layer 3;
[0050] The main body substrate layer 1 includes PET and has a thickness of 200 μm.
[0051] The bridging layer 2 includes 95 parts of polyurethane resin (PU2018 of Guangdong Keding New Materials Co., Ltd.), 5 parts of epoxy resin (X5307 of Guangdong Keding New Materials Co., Ltd.), 5 parts of high carboxyl polyester tackifier (CCK-208K of Huizhou Xiwo Trading Co., Ltd.), 3 parts of silane coupling agent (CCK-310 of Huizhou Xiwo Trading Co., Ltd.), and 15 parts of TDI crosslinking agent (PJ01-50T of Jiangmen Paint Factory Co., Ltd.).
[0052] The hardening layer 3 includes 90 parts of UV polyurethane acrylate (6206C of Guangdong Lan Kelu New Materials Co., Ltd.), 10 parts of UV epoxy resin (6117 of Guangdong Lan Kelu New Materials Co., Ltd.), 4 parts of 184 photoinitiator particles (184 of Guangdong Lan Kelu New Materials Co., Ltd.), 1 part of 1490 photoinitiator particles (1490 of Guangdong Lan Kelu New Materials Co., Ltd.), 0.5 parts of glass fiber reinforced plastic functional particles (EMG11-20 of Shandong Dingshengxi Fiberglass Products Co., Ltd.), and 0.2 parts of antibacterial particle nano zinc oxide (Z-Ink of Guangdong Pugaf Optoelectronics Technology Co., Ltd.).
[0053] Example 4
[0054] This embodiment provides an anti-splash film for glass, comprising a main substrate layer 1, a bridging layer 2 and a hardening layer 3; the bridging layer 2 and the hardening layer 3 are respectively arranged on two sides of the main substrate layer 1.
[0055] The main substrate layer 1 is made of PE and has a thickness of 150 μm.
[0056] The thickness of the bridging layer 2 is 1 μm, and the hardness is HB. The bridging layer 2 includes a main polyurethane resin, a tackifying component, and a crosslinking agent; wherein, it includes 85 parts by weight of a polyurethane resin (PU2018 of Guangdong Keding New Materials Co., Ltd.) and 15 parts by weight of a polyether acrylic resin (B-608 of Guangzhou Jiafucheng Materials Co., Ltd.), the tackifying component includes 1.5 parts by weight of a high-carboxyl polyester tackifying aid (CCK-208K of Huizhou Xiwo Trading Co., Ltd.), and the crosslinking agent includes 15 parts by weight of an isocyanate (3390 of Bayer AG, Germany).
[0057] The thickness of the hardening layer 3 is 3 μm and the hardness is 2H. The hardening layer 3 includes 100 parts by weight of UV polyurethane acrylate (Guangdong Lan Kelu New Materials Co., Ltd. 6206C), 5 parts by weight of 184 photoinitiator particles (Guangdong Lan Kelu New Materials Co., Ltd. 184), 0.2 parts by weight of breathable particles silicone resin microspheres (Japan Shin-Etsu Chemical Co., Ltd. KMP590), 0.2 parts by weight of heat-insulating particles glass fiber reinforced plastic (Shandong Dingshengxi Glass Fiber Products Co., Ltd. EMG11-20) and 0.3 parts by weight of antibacterial particles nano zinc oxide (Guangdong Pujiafu Optoelectronics Technology Co., Ltd. Z-Ink).
[0058] Example 5
[0059] This embodiment provides an anti-splash film for glass, comprising a main substrate layer 1, a bridging layer 2 and a hardening layer 3; the bridging layer 2 and the hardening layer 3 are respectively arranged on two sides of the main substrate layer 1.
[0060] The main substrate layer 1 is made of PP and has a thickness of 200 μm.
[0061] The bridge layer 2 has a thickness of 2 μm and a hardness of H. The bridge layer 2 includes a main polyurethane resin, a tackifying component and a crosslinking agent; wherein the polyurethane resin includes 95 parts by weight of epoxy resin modified polyurethane (MR1762B of Guangdong Keding New Materials Co., Ltd.), 5 parts of epoxy resin (X5307 of Guangdong Keding New Materials Co., Ltd.), the tackifying component includes 1.5 parts by weight of a high carboxyl polyester tackifying aid (CCK-208K of Huizhou Xiwo Trading Co., Ltd.), and the crosslinking agent includes 10 parts by weight of isocyanates (3390 of Bayer AG, Germany).
[0062] The thickness of the hardening layer 3 is 7 μm and the hardness is 4H. The hardening layer 3 includes 90 parts of UV polyurethane acrylate (6206C, Guangdong Lan Kelu New Materials Co., Ltd.), 5 parts of photoinitiator 1490 (1490, Guangdong Lan Kelu New Materials Co., Ltd.), 0.5 parts of breathable particle silicone resin microspheres (KMP590, Shin-Etsu Chemical Co., Ltd., Japan) and 0.2 parts of antibacterial particle nano zinc oxide (Z-Ink, Guangdong Pujiafu Optoelectronics Technology Co., Ltd.).
[0063] Example 6
[0064] This embodiment provides a method for preparing an anti-splash film for glass. Figure 3 , the method for preparing the anti-splash film for glass comprises the following steps:
[0065] Step S1: preparing a bridging layer solution, the specific operation is as follows:
[0066] The polyurethane resin, the tackifying component and the cross-linking agent are mixed according to a mass ratio, diluted with butyl acetate to a desired thickness and solid content, and stirred evenly until a transparent and uniform liquid phase is present to obtain a bridging layer solution.
[0067] Specifically, polyurethane resin (PU2018 of Guangdong Keding New Materials Co., Ltd.), fluorine-containing silicone resin (AD7515W of Guangzhou Keding New Materials Co., Ltd.), biuret crosslinker (TDA-100 of Guangzhou Songwei Trading Co., Ltd.), and high carboxyl polyester tackifier (CCK-208K of Huizhou Xiwo Trading Co., Ltd.) were mixed in a mass ratio of 50:50:15:1.5, diluted with butyl acetate solution to the solid content required for the thickness of the bridging layer, stirred at 600 rpm for 5 minutes using a stirring equipment until a transparent uniform liquid phase was presented, and filtered with a 300-mesh filter for later use.
[0068] Step S2: coating the bridging layer 2 on one side of the main substrate layer 1, the specific operation is as follows:
[0069] The bridging layer solution is coated on the main substrate and dried to obtain a bridging layer 2 on the main substrate. The thickness of the bridging layer 2 is 1-2 μm.
[0070] Specifically, the mixed bridging layer solution was coated on one side of the 200 μm PET main substrate layer 1 with an 80-mesh anilox roller and baked at 120° C. for 5 minutes to obtain the bridging layer 2, and the dry film thickness of the bridging layer 2 was 1-2 μm. After the bridging layer 2 was coated, the film was rolled up so that the bridging layer 2 was located on the inner side of the main substrate layer 1.
[0071] Step S3: preparing a hardening layer solution, the specific operation is as follows:
[0072] The acrylic resin, the photoinitiator and the functional particles are mixed and diluted according to the mass ratio.
[0073] Specifically, UV polyurethane acrylate (6206C from Guangdong Lan Kelu New Materials Co., Ltd.), 184 photoinitiator particles (184 from Guangdong Lan Kelu New Materials Co., Ltd.), and glass 4 fiber reinforced plastic functional particles (EMG11-20 from Shandong Dingshengxi Fiberglass Products Co., Ltd.) were selected, mixed in a mass ratio of 100:5:0.5, and diluted with a solvent to obtain a hardening layer solution.
[0074] Step S4: coating the hardening layer 3 on the side of the main substrate layer 1 away from the bridging layer 2, the specific operation is as follows:
[0075] The hardening layer solution is coated on the side of the main substrate layer 1 away from the cross-linking layer 2, dried, and then irradiated with a UV lamp for curing.
[0076] Specifically, the hardening layer solution is coated on the side of the main substrate layer 1 away from the cross-linking layer 2 by an anilox roller, dried at 90° C. for 5 minutes, and then irradiated with a UV lamp for curing.
[0077] Step S5: Rolling up to obtain the anti-splash film for glass.
[0078] When the anti-splash film for glass is attached to the glass 4, an adhesive layer 5 is provided on the glass 4, and the anti-splash film for glass and the glass 4 are placed in a vacuum negative pressure environment of 0.1MPa to discharge the air, water vapor and small molecule gas dissolved in the adhesive layer 5, so that there are no bubbles between the glass 4 and the anti-splash film for glass after attachment, and the light transmittance is high; the attachment is carried out under a heating state of 130°C, and the glass anti-splash film is fully softened under a high temperature environment, and can be closely attached to the anti-splash film for glass. Since a tackifying component is added to the bridge layer 2 of the anti-splash film for glass, the adhesion between the bridge layer 2 and the adhesive layer 5 is improved, and the peeling strength between the bridge layer 2 and the adhesive layer 5 on the glass 4 can reach 70-100N. When the anti-splash film for glass is attached to the glass 4, the bridge layer 2 is attached to the side of the glass 4, and the hardening layer 3 is located on the side of the main substrate layer 1 away from the bridge layer 2. A construction mold 6 is provided on the hardening layer 3 to keep the anti-splash film for glass, the adhesive layer 5 and the glass 4 fixed, and provide a pressure of 1Mpa to promote the discharge of air in the adhesive layer 5 and the gas between the glass 4 and the anti-splash film for glass. Since the anti-splash film for glass is in a high temperature / high pressure state for a long time during the bonding process, and is attached to the hard construction mold 6, it is inevitable that it will be scratched and adhered to the construction mold 6 when the film is removed, so the hardening layer 3 is provided to provide hardness to achieve the effect of scratch resistance. The hardness of the hardening layer 3 can reach 3H. Under the conditions that the thickness of the hardening layer 3 is close to 5μm and the curling inner diameter of the anti-splash film for glass reaches 3cm, the hardening layer 3 will not burst and fall off, which can not only meet the construction requirements, but also resist the high-speed and high-frequency scratching impact of tiny particles when the vehicle is running at high speed in daily use.
[0079] In one embodiment, the thickness ratio of the glass 4, adhesive layer 5, bridge layer 2, main substrate layer 1, and hardening layer 3 is (500-1000): (80-100): (0.1-0.2): (10-20): (0.3-0.7). Specifically, the glass 4 is 5 mm thick, the adhesive layer 5 is 1 mm thick, the bridge layer 2 is 2 μm thick, the main substrate layer 1 is 200 μm thick, and the hardening layer 3 is 4 μm thick.
[0080] Example 7
[0081] This embodiment provides an anti-splash film for glass, comprising a main substrate layer 1, a bridging layer 2 and a hardening layer 3; the bridging layer 2 and the hardening layer 3 are respectively arranged on two sides of the main substrate layer 1.
[0082] The main substrate layer 1 is made of PET and has a thickness of 100 μm.
[0083] The thickness of the bridge layer 2 is 1 μm, and the hardness is H. The bridge layer 2 includes a main polyurethane resin tackifying component and a crosslinking agent; wherein the polyurethane resin includes 100 parts by weight of epoxy resin modified polyurethane (MR1762B of Guangdong Keding New Materials Co., Ltd.), 3 parts by weight of high carboxyl polyester tackifying aid (CCK-208K of Huizhou Xiwo Trading Co., Ltd.), and the crosslinking agent includes 20 parts by weight of isocyanate (3390 of Bayer, Germany).
[0084] The thickness of the hardening layer 3 is 3 μm and the hardness is 4H. The hardening layer 3 includes 100 parts by weight of UV polyurethane acrylate (Guangdong Lan Kelu New Materials Co., Ltd. 6206C), 8 parts by weight of photoinitiator 1490 (Guangdong Lan Kelu New Materials Co., Ltd. 1490), and 1.5 parts by weight of breathable particle silicone resin microspheres (Japan Shin-Etsu Chemical Co., Ltd. KMP590).
[0085] Example 8
[0086] This embodiment provides an anti-splash film for glass, comprising a main substrate layer 1, a bridging layer 2 and a hardening layer 3;
[0087] The main substrate layer 1 includes PP and has a thickness of 200 μm.
[0088] The bridging layer 2 includes 95 parts by weight of epoxy resin modified polyurethane (MR1762B from Guangdong Keding New Materials Co., Ltd.), 2 parts of silane coupling agent (CCK-310 from Huizhou Xiwo Trading Co., Ltd.), and 15 parts of TDI crosslinking agent (PJ01-50T from Jiangmen Paint Factory Co., Ltd.).
[0089] The hardening layer 3 includes 90 parts of UV polyurethane acrylate (6206C of Guangdong Lan Kelu New Materials Co., Ltd.), 10 parts of UV epoxy resin (6117 of Guangdong Lan Kelu New Materials Co., Ltd.), 4 parts of 184 photoinitiator particles (184 of Guangdong Lan Kelu New Materials Co., Ltd.), 1 part of 1490 photoinitiator particles (1490 of Guangdong Lan Kelu New Materials Co., Ltd.), 0.5 parts of glass fiber reinforced plastic functional particles (EMG11-20 of Shandong Dingshengxi Fiberglass Products Co., Ltd.), and 0.2 parts of antibacterial particle nano zinc oxide (Z-Ink of Guangdong Pugaf Optoelectronics Technology Co., Ltd.).
[0090] Example 9
[0091] This embodiment provides an anti-splash film for glass, including a main substrate layer 1, a bridging layer 2 and a hardening layer 3.
[0092] The main substrate layer 1 includes PP and has a thickness of 200 μm.
[0093] The bridging layer 2 includes 90 parts by weight of epoxy resin modified polyurethane (MR1762B from Guangdong Keding New Materials Co., Ltd.), 10 parts of silane coupling agent (CCK-310 from Huizhou Xiwo Trading Co., Ltd.), and 15 parts of TDI crosslinking agent (PJ01-50T from Jiangmen Paint Factory Co., Ltd.).
[0094] The hardening layer 3 includes 90 parts of UV polyurethane acrylate (6206C of Guangdong Lan Kelu New Materials Co., Ltd.), 10 parts of UV epoxy resin (6117 of Guangdong Lan Kelu New Materials Co., Ltd.), 4 parts of 184 photoinitiator particles (184 of Guangdong Lan Kelu New Materials Co., Ltd.), 1 part of 1490 photoinitiator particles (1490 of Guangdong Lan Kelu New Materials Co., Ltd.), 0.5 parts of glass fiber reinforced plastic functional particles (EMG11-20 of Shandong Dingshengxi Fiberglass Products Co., Ltd.), and 0.2 parts of antibacterial particle nano zinc oxide (Z-Ink of Guangdong Pugaf Optoelectronics Technology Co., Ltd.).
[0095] Comparative Example 1
[0096] This comparative example provides an anti-splash film, comprising a main substrate layer 1, a bridge layer 2 and a hardening layer 3. The bridge layer 2 and the hardening layer 3 are respectively arranged on both sides of the main substrate layer 1;
[0097] The bridging layer 2 includes 97 parts of polyurethane resin (Guangdong Keding New Materials Co., Ltd. PM2018), 3 parts of epoxy resin (Guangdong Keding New Materials Co., Ltd. X5307), 15 parts of TDI crosslinking agent (Jiangmen Paint Factory Co., Ltd. PJ01-50T), and 1 part of high carboxyl polyester tackifier (Huizhou Xiwo Trading Co., Ltd. CCK-208K). Butyl acetate is used as a diluent solvent during mixing.
[0098] The corresponding materials and mass proportions used in the hardening layer 3 are: 80 parts of UV polyurethane acrylate (6206C of Guangdong Lan Kelu New Materials Co., Ltd.), 20 parts of UV epoxy resin (6117 of Guangdong Lan Kelu New Materials Co., Ltd.), 3.5 parts of 184 photoinitiator particles (184 of Guangdong Lan Kelu New Materials Co., Ltd.), and 0.5 parts of 1490 photoinitiator particles (1490 of Guangdong Lan Kelu New Materials Co., Ltd.).
[0099] Relevant performance tests were performed on the anti-splash films of Example 2, Example 3, Example 4, Example 5 and Comparative Example 1, and the test data are shown in Table 1.
[0100] The relevant test contents and methods are as follows: thickness test (GB / T 328.3-2007), hardness test (GB / T6739-2006), abrasion test (GB / T 1768-2006), peel strength test (GB / T 2791-1995), cross-sectional test (GB / T9286-2021), antibacterial test (QB / T 2591-2003), and low temperature resistance test.
[0101] In the low temperature resistance test, two anti-splash films in the large and small embodiments are required in the sample preparation process. The two anti-splash films are respectively attached to the two sides of the PVB layer, and the bridging layer 2 in the anti-splash film is made close to the PVB layer. The areas of the bridging layer 2 and the PVB layer are 10cm*10cm, forming a laminated structure, and placed in a vacuum environment of minus 0.1MPa / 127°C for two hours; after the bonding is completed, it is placed in a -20°C environment for 24 hours to test whether the anti-splash film can be bonded to the PVB layer. If the PVB and the anti-splash film cannot be bonded, the low temperature resistance is judged to be unqualified.
[0102] Table 1 Performance test data table
[0103]
[0104] Please refer to Table 1. In the anti-splash film of comparative example 1, the weight fractions of the cross-linking agent and the thickening component are reduced, resulting in a significant decrease in the peeling performance of the bridging layer 2 and a loss of low-temperature resistance; the weight fraction of the light-initiated particles in the hardening layer 3 is reduced, resulting in a decrease in the surface hardness of the hardening layer 3, and the wear resistance does not meet the requirements, and it does not have antibacterial effect. In the anti-splash films for glass provided in Example 2, Example 3, Example 4, and Example 5, by reasonably matching the types of resin, thickening component, and cross-linking agent, adjusting the corresponding dosage, the peeling strength and low-temperature resistance are improved, and the film has good wear resistance, avoiding wear during processing and damage caused by the impact of fine particles during high-speed driving.
[0105] The present invention is not limited to the above-mentioned embodiments. If various changes or modifications to the present invention do not depart from the spirit and scope of the present invention, and if these changes and modifications fall within the scope of the claims and equivalent technologies of the present invention, the present invention is also intended to include these changes and modifications.
Claims
1. An anti-splash film for glass, characterized in that: It comprises a main substrate layer, a bridging layer and a hardening layer; the bridging layer and the hardening layer are respectively arranged on two sides of the main substrate layer; The bridging layer includes polyurethane resin, tackifying component and crosslinking agent; the polyurethane resin includes one or more of thermoplastic acrylic resin, thermosetting acrylic resin, hydroxy acrylic resin, oil-free polyester resin, fluorine-containing silicone resin and epoxy-modified acrylic resin; the tackifying component includes one or more of high carboxyl polyester, epoxy resin and silane coupling agent; The hardening layer comprises acrylic resin, photoinitiator and functional particles.
2. The anti-splash film for glass according to claim 1, characterized in that: The bridging layer comprises the following components in parts by weight: 90-100 parts by weight of polyurethane resin, 1-10 parts by weight of tackifying component, and 5-20 parts by weight of crosslinking agent; Wherein, the weight portion of the tackifying component is 1-3 parts, and the tackifying component is polyester; or, the weight portion of the tackifying component is 2-10 parts, and the tackifying component is a silane coupling agent.
3. The anti-splash film for glass according to claim 1, characterized in that: The cross-linking agent includes at least one of isocyanate adducts, isocyanate trimers, and biuret adducts.
4. The anti-splash film for glass according to claim 1, characterized in that: The thickness of the bridging layer is 1-2 μm, and the hardness is HB-H.
5. The anti-splash film for glass according to claim 1, characterized in that: In the hardening layer, the acrylic resin includes at least one of UV epoxy acrylate, UV polyurethane acrylate, UV polyester acrylate, and UV pure acrylate.
6. The anti-splash film for glass according to claim 1, characterized in that: The functional particles include at least one of air permeable particles, heat insulating particles and antibacterial particles; The air permeable particles include at least one of inorganic glass and organic resin microspheres, with an average particle size of 0.1 μm; the heat insulating particles include glass fiber reinforced plastics, with an average particle size of 1-1.5 μm; and the antibacterial particles include nano zinc oxide, with an average particle size of 5-10 nm.
7. The anti-splash film for glass according to claim 1, characterized in that: The hardening layer comprises the following components in parts by weight: 90-100 parts by weight of acrylic resin, 3-8 parts by weight of photoinitiator, and 0.3-1.5 parts by weight of functional particles.
8. The anti-splash film for glass according to claim 1, characterized in that: The thickness of the hardened layer is 3-7 μm, and the hardness is 2H-4H.
9. The anti-splash film for glass according to any one of claims 1 to 8, characterized in that: The main substrate layer includes at least one of PET, PE, and PP; The thickness of the main substrate layer is 100-200 μm, and the thickness ratio of the main substrate layer, the bridging layer and the hardening layer is (10-20): (0.1-0.2): (0.3-0.7).
10. A method for preparing the anti-splash film for glass according to any one of claims 1 to 9, characterized in that: The following steps are involved: The polyurethane resin, the tackifying component and the crosslinking agent are mixed according to the mass ratio, and diluted with butyl acetate to the desired thickness of the bridging layer with a solid content of 10%, and stirred evenly until a transparent uniform liquid phase is present to obtain a bridging layer solution; The bridging layer solution is coated on the main substrate and dried to obtain a bridging layer on the main substrate, wherein the thickness of the bridging layer is 1-2 μm; The acrylic resin, the photoinitiator and the functional particles are mixed according to a mass ratio and diluted with butyl acetate to a desired thickness and solid content of the hardening layer to obtain a hardening layer solution; The hardening layer solution is applied to the side of the main substrate away from the bridging layer, dried, and then irradiated with a UV lamp for curing; The anti-splash film for glass is rolled up.
Citation Information
Cited By
Solvent-free preparation method of breakage-proof and splash-proof fabric composite membrane material for glass mirror surface
CN119659043A