Porous framework for preparing directional electromagnetic shielding material as well as preparation method and application of porous framework
Through vacuum sputtering coating process and sensitization activation treatment, a uniform nickel conductive layer is formed, combined with polyimide slurry packaging, the problems of unstable quality of porous skeleton materials and difficulty in wastewater treatment in electromagnetic shielding materials are solved, and high efficiency is achieved Directional electromagnetic shielding performance and low cost production.
Patent Information
- Application Number
- CN202411195236.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The mass of porous skeleton materials in existing electromagnetic shielding materials is greatly affected by the solution concentration during chemical deposition, resulting in unstable electromagnetic shielding performance. The chemical deposition process produces a large amount of wastewater, which is difficult to deal with, making it difficult to meet the needs of directional electromagnetic shielding performance.
The nickel conductive treatment is carried out by vacuum sputtering coating process to form a uniform nickel conductive layer, avoiding the defects of the chemical deposition process, and improving the uniformity and binding force of the nickel conductive layer through sensitization and activation treatment, combining with polyimide Directional electromagnetic shielding materials are prepared for slurry packaging.
The uniformity and stability of the nickel conductive layer are achieved, the wastewater treatment cost is reduced, the conductive performance and directional electromagnetic shielding performance are improved, and the material is efficient and reliable.
Smart Images

Figure CN119081222A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electromagnetic shielding technology, and relates to a porous skeleton used in the preparation process of a double-shielding structural material with directional electromagnetic shielding performance, and applies the porous skeleton to the preparation of a double-shielding structural material with directional electromagnetic shielding performance, and specifically relates to a porous skeleton for preparing a directional electromagnetic shielding material, and a preparation method and application thereof. Background Art
[0002] With the continuous development of aerospace, 5G communication technology, stealth fighters, wearable flexible electronic skin and other technologies, the requirements for electromagnetic shielding, light weight, flexibility and other performance of electromagnetic shielding materials are becoming higher and higher. Polymer materials, as carriers of conductive or magnetic fillers, can reduce the mismatch of the surface impedance of composite materials due to their electrical insulation, making it easier for electromagnetic waves to enter the interior of the composite materials, thereby reducing the reflection and scattering of electromagnetic waves on the surface of the composite materials, playing the role of transmitting electromagnetic waves, and playing the role of electromagnetic wave transmission and absorption in polymer-based electromagnetic shielding composite materials. However, the quality of the electromagnetic shielding effectiveness of polymer composites mainly depends on: (1) the performance of the conductive or magnetic filler itself; (2) whether the conductive or magnetic filler can form a good conductive path between the polymer matrix and have good impedance matching.
[0003] At the same time, with the in-depth study of electromagnetic shielding mechanism by domestic and foreign researchers, it was found that the electromagnetic shielding performance of polymer matrix electromagnetic shielding composite materials also depends on the microstructure of the composite materials, and then the research on the design of composite microstructure to improve electromagnetic shielding performance was carried out to meet the application in different fields. At present, the common microstructures of polymer electromagnetic shielding composite materials mainly include: porous foam structure, multilayer structure, gradient structure, isolation structure, etc. Different microstructures will lead to different electromagnetic wave shielding mechanisms and effects, and composite materials with a single microstructure often do not have directional electromagnetic shielding performance for electromagnetic wave shielding efficiency. Therefore, research and development of electromagnetic shielding materials with directional electromagnetic shielding performance has become a research direction for technicians in this field.
[0004] In order to achieve breakthrough research in this direction, our company has introduced the patented technology of double-shielding structural materials with patent number 202110638506.5, and carried out experimental research on the construction of pilot production lines based on this patented technology. It was found that the quality of porous skeleton materials used in electromagnetic shielding materials is closely affected by the solution concentration during the chemical deposition process, resulting in poor quality stability of porous skeleton materials. For example: in the chemical deposition process of nickel plating, the thickness of the coating will change with the concentration of the chemical plating solution, resulting in poor performance of the electromagnetic shielding material when used to prepare directional electromagnetic shielding materials; and the chemical deposition process produces a large amount of wash water, which requires a wastewater treatment device. Summary of the invention
[0005] Based on the above technical problems, the present invention provides a porous skeleton for preparing directional electromagnetic shielding materials, and a preparation method and application thereof. The porous skeleton material for preparing the electromagnetic shielding material is subjected to conductive nickel plating by a vacuum sputtering coating process, so that the thickness of the nickel layer is more uniform and the quality is more stable. At the same time, it avoids the defects of the chemical deposition process such as large amount of wastewater and difficulty in post-treatment of wastewater.
[0006] The specific technical solution is:
[0007] One of the purposes of the present invention is to provide a method for preparing a conductive porous skeleton for preparing a directional electromagnetic shielding material, comprising the following steps:
[0008] (1) cutting the melamine sponge into suitable sizes, washing and drying, and obtaining a porous skeleton substrate;
[0009] (2) The porous skeleton substrate is subjected to a nickel-plating conductive treatment by vacuum sputtering to obtain a conductive porous skeleton.
[0010] The melamine sponge is cut into suitable sizes, cleaned and dried to form a porous skeleton substrate, and then nickel-plated and conductively treated by a vacuum sputtering coating process. In a vacuum environment, nickel atoms are bombarded from the target material by the sputtering process and deposited on the surface of the porous skeleton substrate to form a uniform nickel conductive layer, thereby achieving conductivity of the porous skeleton substrate and enhancing the stability of the nickel conductive layer. Moreover, the thickness and purity of the nickel conductive layer can be accurately controlled to meet the needs of conductive porous skeletons with different performances.
[0011] In addition, the porous skeleton substrate is treated with nickel for conductivity by vacuum sputtering, which can perform nickel plating at a relatively low temperature, avoiding affecting the performance of the porous skeleton substrate itself and ensuring the stability of the performance of the porous skeleton substrate itself.
[0012] In order to improve the uniformity of the nickel conductive layer on the surface of the porous skeleton substrate, preferably, the vacuum sputtering coating has a sputtering treatment time of 3 minutes, a sputtering vacuum degree of 0.02-0.15 Pa, a sputtering gas flow rate of 0.8-1.5 m / min, and a target-substrate distance of 5-12 cm.
[0013] More preferably, the temperature of the porous skeleton substrate during vacuum sputtering coating is 150°C.
[0014] More preferably, in the vacuum sputtering coating, the target material is metal nickel.
[0015] In order to improve the bonding force between the nickel conductive layer and the surface of the porous skeleton substrate, preferably, the step further includes a porous skeleton substrate sensitization treatment and a porous skeleton substrate activation treatment between the step (1) and the step (2). The porous skeleton substrate sensitization treatment is to immerse the porous skeleton substrate in a sensitizing solution, perform ultrasonic sensitization treatment at room temperature for 30 minutes, and then repeatedly wash it 3 times; the porous skeleton substrate activation treatment is to immerse the porous skeleton substrate in an activation solution, perform ultrasonic activation treatment at room temperature for 30 minutes, and then repeatedly wash it 3 times and then dry it.
[0016] The second purpose of the invention is to provide a conductive porous skeleton prepared by the above method, wherein the nickel conductive layer on the surface of the conductive porous skeleton is evenly distributed and has excellent conductive properties.
[0017] The third purpose of the invention is to provide the conductive porous skeleton prepared by the above method for use in the preparation of double-shielding structural materials with directional electromagnetic shielding performance.
[0018] The preparation of the double-shielding structural material with directional electromagnetic shielding performance comprises the following steps:
[0019] S1: Prepare a conductive porous skeleton according to the above method;
[0020] S2: Preparation of carbon nanotube film with two-dimensional layered structure;
[0021] S3: Encapsulating the conductive porous skeleton and the carbon nanotube membrane with polyimide slurry.
[0022] The conductive porous skeleton is encapsulated with a carbon nanotube membrane using polyimide slurry. Compared with adipic acid / butylene terephthalate, it has better temperature resistance and can work in the range of -200℃ to 400℃. It has a wider temperature range, can ensure excellent encapsulation effect, and improve the overall performance of the material. The specific process of polyimide slurry encapsulation is: align the conductive porous skeleton and the cut carbon nanotube membrane and put them into a suitable container so that the carbon nanotube membrane is under the conductive porous skeleton to obtain a combination; then pour the polyimide slurry into the container so that the combination is completely immersed in the polyimide slurry, and solidify at 180-190℃.
[0023] Compared with the prior art, the technical effects created by the present invention are embodied in:
[0024] The invention utilizes a vacuum sputtering nickel plating process to replace the chemical precipitation nickel plating process in the prior art, thereby promoting uniform distribution of the nickel layer on the conductive porous skeleton, ensuring the stability of product quality, and helping to enhance the conductive properties of the porous skeleton of the nickel conductive layer; and avoids the use of a chemical precipitation nickel plating process, avoids the need to build a back-end sewage treatment device, and reduces the production cost of the conductive porous skeleton. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A process flow diagram is provided for the present invention.
[0026] Figure 2 A schematic diagram of the process flow of another embodiment of the present invention is provided. DETAILED DESCRIPTION
[0027] In order to facilitate those skilled in the art to correctly understand the present invention and enable those skilled in the art to fully understand the technical content of the present invention, the technical solution of the present invention is further explained below in conjunction with specific implementation methods and drawings. However, this explanation does not limit the scope of protection required for the present invention. The scope of protection of the present invention by those skilled in the art cannot be limited to the following explanations. Any equivalent substitutions or changes made by any those skilled in the art or persons familiar with the technology in the art based on the present invention and the technical solution and inventive concept thereof should be covered within the scope of protection of the present invention.
[0028] like Figure 1 As shown, in some embodiments, a method for preparing a conductive porous skeleton for preparing a directional electromagnetic shielding material includes: cutting a melamine sponge into a suitable size, washing and drying, and obtaining a porous skeleton substrate; and performing a nickel-plating conductive treatment on the porous skeleton substrate by vacuum sputtering to obtain a conductive porous skeleton. The vacuum sputtering nickel plating treatment forms a stable and uniform nickel conductive layer on the surface of the porous skeleton substrate, thereby improving the conductive properties of the conductive porous skeleton; the need to install a wastewater treatment device at the back end of the process in the chemical deposition nickel plating process is avoided, thereby reducing the cost of the conductive treatment of the melamine sponge and ensuring the quality of the conductive treatment.
[0029] In some embodiments, the vacuum sputtering coating has a sputtering treatment time of 3 minutes, a sputtering vacuum degree of 0.02-0.15 Pa, a sputtering gas flow rate of 0.8-1.5 m / min, a target-substrate distance of 5-12 cm, a temperature of 150° C. during the vacuum sputtering coating, and a target material of nickel. The conductivity of the conductive porous skeleton is maintained at 310.2-337.6 S / m.
[0030] like Figure 2As shown, in some embodiments, the steps further include sensitizing the porous skeleton substrate and activating the porous skeleton substrate, and then conducting the porous skeleton substrate. The porous skeleton substrate sensitization treatment is to immerse the porous skeleton substrate in a sensitizing solution, ultrasonically sensitize it for 30 minutes at room temperature, and then wash it repeatedly for 3 times; the porous skeleton substrate activation treatment is to immerse the porous skeleton substrate in an activation solution, ultrasonically activate it for 30 minutes at room temperature, and then wash it repeatedly for 3 times and dry it. It helps to improve the uniformity of the nickel plating layer on the porous skeleton, improve the quality stability of the conductive porous skeleton product, and enhance the conductive performance of the conductive porous skeleton.
[0031] In some embodiments, the preparation of a double shielding structure material having directional electromagnetic shielding performance comprises the following steps:
[0032] S1: Prepare a conductive porous skeleton according to the above method;
[0033] S2: Preparation of carbon nanotube film with two-dimensional layered structure;
[0034] S3: Encapsulating the conductive porous skeleton and the carbon nanotube membrane with polyimide slurry.
[0035] Using polyimide slurry as the packaging material for the conductive porous skeleton and carbon nanotube membrane encapsulation fully utilizes the wide working temperature range of polyimide slurry, reduces the difficulty of encapsulation processing, and at the same time improves the temperature resistance of the product and ensures the stability of the product application performance. The specific packaging process is to align the conductive porous skeleton and the cut carbon nanotube membrane and put them into a suitable container so that the carbon nanotube membrane is under the conductive porous skeleton to obtain a combination; then pour the polyimide slurry into the container so that the combination is completely soaked in the polyimide slurry and then take it out and cure it at 180-190℃.
[0036] In order to verify the technical effect that the present invention can bring, the research team of the present invention conducted a pilot test on the double-shielding structure material technology with the introduced patent number 202110638506.5, and on the basis of this patented technology, avoided the defect of high cost caused by the chemical deposition nickel plating process that requires the installation of a back-end wastewater treatment device, and conducted improvement research on the porous skeleton conductive treatment process, and conducted corresponding laboratory research. The following is an explanation of the research content.
[0037] Experiment 1: Experimental study on the effects of different treatment processes on the performance of porous skeleton conductive products.
[0038] Example 1
[0039] like Figure 1As shown, the melamine sponge sold on the market was cut into 3cm×2.5cm×0.3cm, put into an ultrasonic cleaning machine for ultrasonic (30kHz) cleaning (deionized water) for 5min, cleaned three times in a row, and dried to obtain a porous skeleton substrate; the porous skeleton substrate was placed in a magnetron sputtering device, under a vacuum (0.1Pa) environment, with metal nickel as the target material and argon as the sputtering gas flow, the distance between the target material and the porous skeleton substrate was controlled to be 10cm, the sputtering temperature was controlled to be 150°C, the sputtering gas flow rate was 1m / min, and the sputtering treatment was performed for 3min to obtain a conductive porous skeleton.
[0040] Example 2
[0041] like Figure 2 As shown, on the basis of Example 1, the porous skeleton substrate is immersed in a sensitizing solution (2g of stannous chloride and 1mL of concentrated hydrochloric acid are added to 100mL of deionized water), and is subjected to ultrasonic (30kHz) sensitization treatment for 30min at room temperature (25°C), and then repeatedly washed with deionized water for 3 times; then immersed in an activation solution (10mg of palladium chloride and 0.1ml of concentrated hydrochloric acid are added to 100ml of deionized water), and is subjected to ultrasonic (30kHz) activation treatment for 30min at room temperature (25°C), and is repeatedly washed with deionized water for 3 times, and then dried; and placed in a magnetron sputtering device for vacuum sputtering nickel plating treatment according to the vacuum sputtering process of Example 1 to obtain a conductive porous skeleton.
[0042] Example 3
[0043] like Figure 1 As shown, on the basis of Example 1, the vacuum degree is 0.02 Pa, the distance between the target material and the porous skeleton substrate is controlled to be 5 cm, the sputtering temperature is controlled to be 150°C, the sputtering gas flow rate is 1.5 m / min, and the rest are the same as Example 1, to obtain a conductive porous skeleton.
[0044] Example 4
[0045] like Figure 1 As shown, on the basis of Example 1, the vacuum degree is 0.15 Pa, the distance between the target material and the porous skeleton substrate is controlled to be 12 cm, the sputtering temperature is controlled to be 150°C, the sputtering gas flow rate is 0.8 m / min, and the rest are the same as Example 1, to obtain a conductive porous skeleton.
[0046] Example 5
[0047] like Figure 1 As shown, on the basis of Example 1, the vacuum degree is 0.08 Pa, the distance between the target material and the porous skeleton substrate is controlled to be 8 cm, the sputtering temperature is controlled to be 150°C, the sputtering gas flow rate is 0.5 m / min, and the rest are the same as Example 1, to obtain a conductive porous skeleton.
[0048] The conductive porous skeletons prepared in Examples 1 to 5 were tested for their conductive properties (conductivity, with one decimal place retained), and the conductive porous skeletons prepared in each Example were cut into 3 sections on average, i.e., 1.0 cm × 2.5 cm × 0.3 cm in size, labeled A, B, C, and weighed and recorded as M. A 、M B 、M C , calculate the weight change rate between the three sections (keep five decimal places), the calculation method is as follows:
[0049] Calculation of weight change rate of A relative to B (Y A→B ): [(M A -M B )÷M B ]×100%;
[0050] Calculation of weight change rate of A relative to C (Y A→C ): [(M A -M C )÷M C ]×100%;
[0051] Calculation of weight change rate of B relative to C (Y B→C ): [(M B -M C )÷M C ]×100%.
[0052] The data of each example was tested three times and the average value was recorded. The calculation results are shown in Table 1.
[0053] Table 1
[0054]
[0055] As shown in Table 1, the invention uses a vacuum sputtering process to plate nickel on the melamine sponge, which can help improve the uniformity of the nickel plating layer, thereby improving the conductivity of the conductive porous skeleton. It is also found that after the melamine sponge is treated with a sensitizing liquid for sensitization and an activating liquid for sensitization, it will help improve the uniformity of the nickel layer covering the melamine sponge, thereby improving the conductivity of the conductive porous skeleton.
[0056] Experiment 2: Experimental study on the use of conductive porous skeletons obtained by different processes to prepare directional electromagnetic shielding materials.
[0057] The conductive porous skeleton material prepared in Example 1-5 of Experiment 1 and the cut carbon nanotube film are aligned and placed in a suitable container (e.g., a culture dish) so that the carbon nanotube film is below the conductive porous skeleton to obtain a composite body; polyimide slurry is then poured into the container so that the composite body is completely soaked in the polyimide slurry and then taken out and cured at a temperature between 180-190°C to obtain a directional electromagnetic shielding material. The average EMI SE of the directional electromagnetic shielding material in the X-band is measured by injecting electromagnetic waves from the front and back sides respectively. T The results are shown in Table 2 below.
[0058] Table 2
[0059]
[0060] As shown in Table 2, the conductive porous skeleton is prepared by vacuum sputtering process, and then the conductive porous skeleton is used to prepare electromagnetic shielding material. T There are obvious differences, and different vacuum sputtering processes will lead to material EMI SE T Different from the above, the melamine sponge is treated with sensitizing liquid and activating liquid, which can significantly improve the EMI SE of the material. T The anisotropy of the material will determine the different electromagnetic wave losses due to different electromagnetic wave injection paths, making it have directional electromagnetic shielding performance.
[0061] The present invention creates a porous skeleton substrate (melamine sponge) that is conductively treated by a vacuum sputtering process, which not only avoids the defect of high cost of post-processing equipment in the prior art for conductively treating porous skeleton substrates using a chemical deposition process, but also can enhance the difference in isotropic shielding of electromagnetic waves of the directional electromagnetic shielding material to a certain extent after the conductively treated porous skeleton is applied to the preparation of the directional electromagnetic shielding material with reference to the prior art (for example: the technology disclosed in Patent No. 202110638506.5), thereby enhancing the performance of the material in directional shielding of electromagnetic waves.
[0062] Other matters not covered in the present invention may be achieved by conventional technical means with reference to the prior art or common knowledge known to those skilled in the art. For example, the carbon nanotube film used in the embodiments of the present invention is prepared with reference to the technology disclosed in Patent No. 202110638506.5. Another example: the drying temperature in the present invention refers to the drying treatment in a vacuum oven at 40°C disclosed in Patent No. 202110638506.5. Another example: the polyimide slurry used in the present invention is a slurry commonly used by those skilled in the art, such as yellow polyimide slurry (YPI) and the like.
Claims
1. A method for preparing a conductive porous skeleton for preparing a directional electromagnetic shielding material, characterized in that: The following steps are involved: (1) cutting the melamine sponge into suitable sizes, washing and drying, and obtaining a porous skeleton substrate; (2) The porous skeleton substrate is subjected to a nickel-plating conductive treatment by vacuum sputtering to obtain a conductive porous skeleton.
2. The method for preparing a conductive porous skeleton for preparing a directional electromagnetic shielding material according to claim 1, characterized in that: The vacuum sputtering coating has a sputtering treatment time of 3 minutes, a sputtering vacuum degree of 0.02-0.15 Pa, a sputtering gas flow velocity of 0.8-1.5 m / min, and a target-base distance of 5-12 cm.
3. The method for preparing a conductive porous skeleton for preparing a directional electromagnetic shielding material according to claim 1, characterized in that: The temperature of the porous skeleton substrate during vacuum sputtering coating is 150°C.
4. The method for preparing a conductive porous skeleton for preparing a directional electromagnetic shielding material according to claim 1, 2 or 3, characterized in that: In the vacuum sputtering coating, the target material is metal nickel.
5. The method for preparing a conductive porous skeleton for preparing a directional electromagnetic shielding material according to claim 1, characterized in that: The steps also include a porous skeleton substrate sensitization treatment and a porous skeleton substrate activation treatment between the steps (1) and (2).
6. The method for preparing a conductive porous skeleton for preparing a directional electromagnetic shielding material according to claim 5, characterized in that: The porous skeleton substrate sensitization treatment is to immerse the porous skeleton substrate in a sensitizing solution, perform ultrasonic sensitization treatment at room temperature for 30 minutes, and then wash it repeatedly for 3 times; the porous skeleton substrate activation treatment is to immerse the porous skeleton substrate in an activation solution, perform ultrasonic activation treatment at room temperature for 30 minutes, and then wash it repeatedly for 3 times and then dry it.
7. A conductive porous skeleton prepared by the method according to any one of claims 1 to 6.
8. Use of the conductive porous skeleton prepared by the method according to any one of claims 1 to 6 in the preparation of double-shielding structural materials with directional electromagnetic shielding performance.
9. The use according to claim 8, characterized in that The preparation of the double shielding structure material with directional electromagnetic shielding performance, The following steps are involved: S1: preparing a conductive porous skeleton according to the method according to any one of claims 1 to 6; S2: Preparation of carbon nanotube film with two-dimensional layered structure; S3: Encapsulating the conductive porous skeleton and the carbon nanotube membrane with polyimide slurry.
10. The use according to claim 9, characterized in that: The step S3 is: aligning the conductive porous skeleton and the cut carbon nanotube membrane and placing them in a suitable container so that the carbon nanotube membrane is below the conductive porous skeleton to obtain an assembly; then pouring polyimide slurry into the container so that the assembly is completely immersed in the polyimide slurry, and curing at 180-190°C.