Sizing material with biomass reinforcing agent applied to liquid reclaimed rubber and preparation method of sizing material
By mixing the lignin composition modified with liquid recycled rubber, the problem of poor compatibility and dispersion in rubber is solved, the processing performance and added value of the rubber is improved, and the better Reinforcement effect.
Patent Information
- Application Number
- CN202411172602.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-06
AI Technical Summary
Lignin has poor compatibility and dispersion in rubber, resulting in poor reinforcement effect.
The lignin composition is modified with a silane coupling agent and mixed with liquid regenerated rubber, and treated by a screw extruder to improve compatibility and dispersion, while partially replacing carbon black and rubber additives to improve the gel Processing performance.
It improves the compatibility and dispersion of lignin and recycled rubber, reduces the use of carbon black, improves the processing performance and added value of rubber, and enhances the value of rubber semi-products.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials, and in particular to a rubber material in which a biomass reinforcing agent is applied to liquid regenerated rubber and a preparation method thereof. Background Art
[0002] Commonly used rubber reinforcing agents include carbon black, white carbon black, clay and other inorganic fillers, most of which are derived from minerals and are non-renewable substances. As human beings' understanding of environmental pollution and resource crises continues to deepen, more and more people are aware of the importance of using materials with renewable and degradable properties. Therefore, lignin as a rubber reinforcing agent has also received more and more attention.
[0003] Lignin is a type of heterogeneous complex cross-linked organic polymer that exists in wood tissues. It forms relatively hydrophobic aromatic phenylpropanoid supplements with cellulose and hemicellulose in the structural components of vascular plants, located between fibers and playing a compressive role. Because its molecular structure contains many active functional groups such as conjugated double bonds, aromatic groups, phenolic hydroxyl groups, alcoholic hydroxyl groups, carbonyl groups, methoxyl groups and carboxyl groups, and it also has the advantages of being renewable, non-toxic and widely available, it is increasingly used in rubber.
[0004] Liquid rubber is a material with a certain fluidity at room temperature. After the waste rubber is mixed with a regenerating agent and then treated by heating or other methods, the resulting liquid regenerated rubber can not only promote the reuse of waste rubber, but also partially replace some additives in the rubber composition. Liquid regenerated rubber has good processing properties, is helpful for the dispersion of fillers and the improvement of the performance of rubber compositions, and has been widely used in various fields.
[0005] The application of lignin in rubber compositions has been mentioned in many patents. The patent (CN202011583948.6 A modified lignin and its preparation method and its application in rubber composite materials) proposes a method of reacting lignin with an acetylenic compound in an organic solvent to obtain a reaction solution containing modified lignin, and mixing the modified lignin with natural rubber and carbon black to obtain a mixed rubber, which reduces the polarity of the molecule, inhibits the self-aggregation tendency of lignin caused by hydrogen bonds, is conducive to grinding to obtain lignin powder with a lower particle size, improves the compatibility and affinity of lignin with non-polar natural rubber, and promotes the dispersion of lignin in the rubber matrix. The patent (CN202010484885.2 A modified lignin-enhanced rubber and its preparation method) proposes a modified lignin-enhanced rubber and its preparation method, wherein the modified lignin is prepared by composite modification of a compound containing a carbon-carbon double bond, a compound containing a sulfur element, and a compound capable of blocking a hydroxyl group. However, due to the presence of polar functional groups such as hydroxyl and carboxyl in lignin, it has poor compatibility and dispersibility in the rubber matrix, resulting in poor reinforcement effect. Summary of the invention
[0006] The present invention provides a rubber material and a preparation method for a biomass reinforcing agent used in liquid reclaimed rubber, in an effort to solve or at least alleviate at least one of the above problems.
[0007] The present invention provides a method for preparing a rubber compound by applying a biomass reinforcing agent to liquid reclaimed rubber, characterized in that the method comprises:
[0008] After uniformly mixing the waste rubber powder and the regenerating agent, the waste rubber powder is added to the first screw extruder, the temperature of different sections of the first screw extruder is controlled at 170°C to 320°C, and after reacting for 2 to 5 minutes, the waste rubber powder is sent to the second screw extruder through a continuous conveying device, and the prefabricated lignin composition is added through a side feeding device, and the temperature of the second screw extruder is controlled at 140°C to 160°C. After reacting for 2 to 4 minutes, the waste rubber powder is discharged to obtain liquid regenerated rubber, wherein the sol content is greater than 75%, and the number average molecular weight Mn is 6000 to 18000;
[0009] 100 parts by mass of raw rubber, 40-70 parts of the liquid regenerated rubber, 20-50 parts of carbon black, 2-5 parts of sulfur, 2-10 parts of softener, 1-5 parts of antioxidant and 2-6 parts of accelerator are added into an internal mixer, mixed for 3-8 minutes and then discharged to obtain the rubber material.
[0010] As a preferred embodiment of the present invention, the waste rubber powder includes any one or more combinations of waste tire rubber powder, waste EPDM rubber, and waste butyl rubber; the regeneration agent includes a softener and an activator; the softener is any one or more combinations of pine tar pitch, tall oil pitch, and rosin; the activator is a disulfide; the weight ratio of the waste rubber powder to the softener and the activator is 100:(3-8):(0.5-4).
[0011] As a preferred embodiment of the present invention, the first screw extruder is a twin-screw extruder with a length-to-diameter ratio of (40-52):1, a screw speed of 220-300 rpm, a heating section temperature of 180°C-250°C, a reaction section temperature of 250°C-320°C, and a cooling section temperature of 170°C-220°C.
[0012] As a preferred embodiment of the present invention, the second screw extruder is a twin-screw extruder with a length-to-diameter ratio of (32-44):1 and a screw speed of 140-200 rpm.
[0013] As a preferred embodiment of the present invention, the preparation method of the lignin composition comprises:
[0014] Obtaining industrial lignin extracted by pulping process on a large scale, wherein the industrial lignin includes: any one or more combinations of kraft lignin, lignin sulfonate, alkali lignin and organic solvent lignin;
[0015] The industrial lignin, natural rubber and silane coupling agent are added into an internal mixer in a mass fraction ratio of (30-60):100:(10-25), mixed for 3-6 minutes and then discharged to obtain the lignin composition modified by the silane coupling agent, wherein the silane coupling agent is any one or more of KH560, KH570 and KH550.
[0016] As a preferred embodiment of the present invention, the raw rubber includes: any one or more combinations of natural rubber, butadiene rubber, styrene-butadiene rubber, and butyl rubber.
[0017] As a preferred embodiment of the present invention, the carbon black comprises any one or more combinations of carbon black N330, carbon black N660, and carbon black N550.
[0018] As a preferred embodiment of the present invention, the softener comprises: any one or more combinations of aromatic oil, pine tar oil, tall oil, and naphthenic oil.
[0019] As a preferred embodiment of the present invention, the antioxidant includes: any one or more combinations of antioxidant 4010, antioxidant 4020, and antioxidant 2246.
[0020] As a preferred embodiment of the present invention, the accelerator comprises: any one or more combinations of accelerator TMTD, accelerator DZ, and accelerator DM.
[0021] The present invention provides a rubber material in which a biomass reinforcing agent is applied to liquid regenerated rubber. The rubber material is prepared by a method for preparing a rubber material in which the biomass reinforcing agent provided by the present invention is applied to liquid regenerated rubber.
[0022] Compared with the prior art, the present invention has at least the following beneficial effects:
[0023] In view of the poor compatibility between lignin and rubber, the present invention proposes to use a silane coupling agent as a bridge between rubber and lignin, first prefabricate a lignin composition, and then apply it to liquid regenerated rubber, which not only improves the compatibility and dispersibility between lignin and regenerated rubber, but also reduces the use of carbon black in rubber by using lignin as a partial substitute for carbon black. At the same time, various rubber additives in the liquid regenerated rubber are added to the rubber composition, which can partially replace softeners and plasticizers, thereby increasing the value of rubber semi-finished products and improving the processing performance of rubber compounds.
[0024] At the same time, in the present invention, the industrial by-product lignin is effectively utilized, thereby increasing its added value; the prefabricated lignin composition reduces the difficulty of adding materials to a screw extruder, while promoting further mixing of lignin in liquid regenerated rubber, thereby increasing its dispersibility and uniformity of the rubber; various rubber additives in the liquid regenerated rubber are added to the rubber composition, thereby partially replacing softeners and plasticizers, thereby increasing the value of the rubber compound. DETAILED DESCRIPTION
[0025] Exemplary embodiments of the present invention will be described in more detail below. Although exemplary embodiments of the present invention have been shown, it should be appreciated that the present invention can be realized in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to more thoroughly understand the present invention, and the scope of the present invention can be fully communicated to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0026] Example 1
[0027] After uniformly mixing the waste tire rubber powder and the regenerating agent, add them to the first screw extruder, control the temperature of different sections of the extruder at 170℃-320℃, react for 3 minutes under the heat and high shear of the screw, and send them to the second screw extruder through a continuous conveying device, add the prefabricated lignin composition through a side feeding device, control the temperature of the extruder at 145℃, and discharge after 3 minutes to obtain liquid regenerated rubber, whose sol content is greater than 75% and the number average molecular weight Mn is 11380. 100 parts by mass of natural rubber, 55 parts of the prepared liquid regenerated rubber, 35 parts of carbon black N330, 2 parts of sulfur, 5 parts of softener aromatic oil, 5 parts of antioxidant 4010, and 3 parts of accelerator TMTD are added to an internal mixer, mixed for 4 minutes and discharged to obtain the desired rubber.
[0028] The preparation steps of the prefabricated lignin composition are as follows: natural rubber, sulfate lignin, and silane coupling agent KH550 are added into an internal mixer according to a mass fraction ratio of 100:35:16, mixed for 4 minutes, and discharged to obtain a silane coupling agent-modified lignin composition.
[0029] Example 2
[0030] After uniformly mixing the waste tire rubber powder and the regenerating agent, add them to the first screw extruder, control the temperature of different sections of the extruder at 170℃-320℃, react for 4 minutes under the heat and high shear of the screw, and send them to the second screw extruder through a continuous conveying device, add the prefabricated lignin composition through a side feeding device, control the temperature of the extruder at 150℃, and discharge after 4 minutes to obtain liquid regenerated rubber, whose sol content is greater than 75% and the number average molecular weight Mn is 10894. 100 parts by mass of natural rubber, 50 parts of the prepared liquid regenerated rubber, 38 parts of carbon black N330, 3 parts of sulfur, 4 parts of softener aromatic oil, 4 parts of antioxidant 4020, and 3 parts of accelerator DZ are added to an internal mixer, mixed for 5 minutes and discharged to obtain the desired rubber.
[0031] The preparation steps of the prefabricated lignin composition are as follows: natural rubber, alkali lignin, and silane coupling agent KH550 are added into an internal mixer in a mass fraction ratio of 100:40:10, mixed for 4 minutes, and discharged to obtain a silane coupling agent-modified lignin composition.
[0032] Example 3
[0033] After uniformly mixing the waste tire rubber powder and the regenerating agent, add them to the first screw extruder, control the temperature of different sections of the extruder at 170℃-320℃, react for 4 minutes under the heat and high shear of the screw, and send them to the second screw extruder through a continuous conveying device, add the prefabricated lignin composition through a side feeding device, control the temperature of the extruder at 153℃, and discharge after 3 minutes to obtain liquid regenerated rubber, whose sol content is greater than 75% and the number average molecular weight Mn is 9279. 100 parts by mass of natural rubber, 50 parts of the prepared liquid regenerated rubber, 43 parts of carbon black N330, 4 parts of sulfur, 4 parts of softener tall oil, 4 parts of antioxidant 2246, and 3 parts of accelerator DM are added to an internal mixer, mixed for 5 minutes and discharged to obtain the desired rubber.
[0034] The preparation steps of the prefabricated lignin composition are as follows: natural rubber, sulfate lignin, and silane coupling agent KH550 are added into an internal mixer in a mass fraction ratio of 100:45:18, kneaded for 4 minutes, and discharged to obtain a silane coupling agent-modified lignin composition.
[0035] The results of the above-mentioned Example 1, Example 2 and Example 3 are shown in the following table:
[0036] Vulcanization: 140℃×20min Example 1 Example 2 Example 3 Tensile strength / MPa 18.4 17.2 17.6 300% elongation / MPa 10.3 10.5 10.9 Elongation at break / % 513 524 528 Hardness / Shore A 57 59 60
[0037] It should be understood that in order to streamline the present invention and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, the various features of the present invention are sometimes grouped together into a single embodiment, or description thereof. However, this method of invention should not be interpreted as reflecting the intention that the claimed invention requires more features than those explicitly recited in each claim. More specifically, as reflected in the claims below, inventive aspects lie in less than all of the features of a single embodiment of the preceding invention. Therefore, the claims that follow the specific embodiment are hereby expressly incorporated into the specific embodiment, with each claim itself serving as a separate embodiment of the present invention.
[0038] In addition, those skilled in the art will appreciate that, although some embodiments described herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and form different embodiments. For example, in the claims, any one of the claimed embodiments may be used in any combination.
[0039] The above description is only an illustrative embodiment of the present invention and is not intended to limit the present invention in any form or substance. It should be pointed out that, for ordinary technicians in this technical field, a number of improvements and supplements made without departing from the method of the present invention should also be regarded as the protection scope of the present invention; any equivalent changes, modifications and evolutions made by technicians familiar with this profession using the technical content disclosed above without departing from the spirit and scope of the present invention are all equivalent embodiments of the present invention; at the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention still fall within the protection scope of the present invention.
Claims
1. A method for preparing rubber material by using a biomass reinforcing agent in liquid reclaimed rubber, It is characterized in that The method includes: After uniformly mixing the waste rubber powder and the regenerating agent, the waste rubber powder is added to the first screw extruder, the temperature of different sections of the first screw extruder is controlled at 170°C to 320°C, and after reacting for 2 to 5 minutes, the waste rubber powder is sent to the second screw extruder through a continuous conveying device, and the prefabricated lignin composition is added through a side feeding device, and the temperature of the second screw extruder is controlled at 140°C to 160°C. After reacting for 2 to 4 minutes, the waste rubber powder is discharged to obtain liquid regenerated rubber, wherein the sol content is greater than 75%, and the number average molecular weight Mn is 6000 to 18000; 100 parts by mass of raw rubber, 40-70 parts of the liquid regenerated rubber, 20-50 parts of carbon black, 2-5 parts of sulfur, 2-10 parts of softener, 1-5 parts of antioxidant and 2-6 parts of accelerator are added into an internal mixer, mixed for 3-8 minutes and then discharged to obtain the rubber material.
2. A method for preparing rubber material by using the biomass reinforcing agent in liquid reclaimed rubber according to claim 1, It is characterized in that The waste rubber powder includes: any one or more combinations of waste tire rubber powder, waste EPDM rubber and waste butyl rubber; the regeneration agent includes: a softener and an activator; the softener is any one or more combinations of pine tar pitch, tall oil pitch and rosin; the activator is a disulfide; the weight ratio of the waste rubber powder to the softener and the activator is 100:3-8:0.5-4.
3. A method for preparing rubber material by using the biomass reinforcing agent in liquid reclaimed rubber according to claim 1, It is characterized in that The first screw extruder is a twin-screw extruder with a length-to-diameter ratio of 40 to 52:1, a screw speed of 220 to 300 rpm, a heating section temperature of 180 to 250°C, a reaction section temperature of 250 to 320°C, and a cooling section temperature of 170 to 220°C.
4. A method for preparing rubber material by using the biomass reinforcing agent in liquid reclaimed rubber according to claim 1, It is characterized in that The second screw extruder is a twin-screw extruder with a length-to-diameter ratio of 32 to 44:1 and a screw speed of 140 to 200 rpm.
5. A method for preparing rubber material by using the biomass reinforcing agent in liquid reclaimed rubber according to claim 1, It is characterized in that The preparation method of the lignin composition comprises: Obtaining industrial lignin extracted by pulping process on a large scale, wherein the industrial lignin includes: any one or more combinations of kraft lignin, lignin sulfonate, alkali lignin and organic solvent lignin; The industrial lignin, natural rubber and silane coupling agent are added into an internal mixer in a mass fraction ratio of 30-60:100:10-25; after mixing for 3-6 minutes, the material is discharged to obtain the lignin composition modified by the silane coupling agent, wherein the silane coupling agent is any one or more combinations of KH560, KH570 and KH550.
6. A method for preparing rubber material by using the biomass reinforcing agent in liquid reclaimed rubber according to claim 1, It is characterized in that The raw rubber includes any one or more combinations of natural rubber, butadiene rubber, styrene-butadiene rubber and butyl rubber.
7. A method for preparing rubber material by using the biomass reinforcing agent in liquid reclaimed rubber according to claim 1, It is characterized in that The carbon black includes: any one or more combinations of carbon black N330, carbon black N660 and carbon black N550.
8. A method for preparing rubber material by using the biomass reinforcing agent in liquid reclaimed rubber according to claim 1, It is characterized in that The softener comprises: a combination of any one or more of aromatic oil, pine tar oil, tall oil and naphthenic oil.
9. A method for preparing rubber material by using the biomass reinforcing agent in liquid reclaimed rubber according to any one of claims 1 to 8, It is characterized in that The antioxidant includes: antioxidant 4010, antioxidant 4020, and antioxidant 2246, any one or more combinations thereof.
10. A biomass reinforcing agent is used in a rubber compound in liquid reclaimed rubber. It is characterized in that The rubber compound is prepared by the method for preparing the rubber compound by applying the biomass reinforcing agent described in any one of claims 1 to 9 to liquid regenerated rubber.
Citation Information
Patent Citations
Modified lignin enhanced rubber and preparation method thereof
CN111533922A
Modified lignin as well as preparation method and application thereof in rubber composite material
CN112831059A
Silane coupling agent modified hydroxymethyl lignin filled rubber composition and preparation method thereof
CN103951858A
Pulverization modified lignin, preparation method and applications thereof
CN104830081A
Tire sidewall rubber material containing liquid reclaimed rubber and preparation method thereof
CN113278206A
Cited By
Method for preparing high-strength rubber through co-regeneration of waste wind power blades and waste tires
CN121779800A