HIPS (High Impact Polystyrene) alloy material as well as preparation method and application thereof
By adding specific hollow glass microbeads and ASA glue powder to the HIPS material, combined with phosphorus and nitrogen flame retardants, the shortcomings of thin-walled HIPS materials in the 5VA flame retardant grade and toughness are solved, and 5VA is achieved without halogen The combination of flame retardant and excellent mechanical properties reduces production costs.
Patent Information
- Application Number
- CN202411276689.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The existing HIPS materials are difficult to meet the 5VA flame retardant grade in the thin-walled state, and there are toughness and cost problems. Traditional flame retardants are threats to the environment and affect mechanical properties.
By adding hollow glass microbeads with a specific average particle size range and ASA powder with a specific acrylate content to the HIPS alloy material, and combining phosphorus and nitrogen flame retardants, the bridge is formed to improve binding force and flame retardant performance. Use compatibilizers to improve system compatibility and prepare thin-walled products with halogen-free 5VA flame retardant grade.
It is achieved that the thin-walled HIPS material reaches a 5VA flame retardant level without adding anti-drip agent, while improving the toughness and rigidity of the material, reducing density and production costs, and having excellent mechanical properties and flame retardant properties.
Smart Images

Figure BDA0005040403870000071 
Figure BDA0005040403870000081 
Figure BDA0005040403870000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer engineering plastics, and in particular relates to a HIPS alloy material and a preparation method and application thereof. Background Art
[0002] GPPS, or general purpose polystyrene, is a general purpose plastic with the advantages of high rigidity, high gloss, high flow and dimensional stability. It is widely used in home appliances, office equipment, automobiles and other fields, but its toughness is poor, which limits its application in fields with high toughness requirements. At present, the most common way to improve the defect of poor impact performance of general purpose polystyrene is to modify general purpose polystyrene by adding polybutadiene rubber to form high impact polystyrene (HIPS). The improvement of toughness has greatly broadened the application range of PS materials, but HIPS itself is a flammable material, which is easy to drip and burn through during the combustion process, so it cannot meet the 5VA flame retardant grade. Usually, a considerable proportion of bromine antimony flame retardant and anti-dripping agent must be added to have a 5VA flame retardant grade. However, brominated flame retardants and anti-dripping agents (commonly used polytetrafluoroethylene) have two major problems: high price and environmental protection.
[0003] At present, thin-walling (thickness ≤ 2mm) has become the development trend of many products, such as televisions, printers and car interiors, which leads to higher and higher requirements for flame retardant properties. Since 5VA flame retardancy is higher than V-0 flame retardancy, meeting 5VA flame retardancy has also become an important development direction for many materials to meet the requirements for high flame retardancy after thin-walling of products. Chinese patent (CN112745591B) discloses a flame retardant high-rigidity PS / PPE composite material and its preparation. The scheme adopts brominated flame retardant and glass fiber compound to achieve 5VA flame retardant grade, but the use of brominated flame retardant cannot meet the halogen-free environmental protection requirements, and the patent does not explore whether the thin-walled product can still meet the 5VA flame retardant grade. Chinese patent (CN117757208A) discloses a polystyrene material, which can achieve a 5VA flame retardant grade for products with a thickness of 2mm, but it adds an anti-dripping agent to the formula, which not only threatens the environment, but also damages the mechanical properties to a certain extent. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a HIPS alloy material that can meet the 5VA flame retardant grade in a thin-walled state (thickness ≤ 2 mm) and has good strength and toughness, as well as a preparation method and application thereof.
[0005] To achieve the above object, in a first aspect of the present invention, the present invention provides a HIPS alloy material, wherein the HIPS alloy material comprises the following components in parts by mass: 58-82 parts of HIPS resin, 18-42 parts of ASA rubber powder, 10-18 parts of phosphorus flame retardant, 3-9 parts of nitrogen flame retardant, 4-12 parts of hollow glass microspheres, and 1-9 parts of compatibilizer;
[0006] In the ASA rubber powder, the mass content of acrylate is 53-66%;
[0007] The average particle size of the hollow glass microspheres is 38-82 μm.
[0008] A HIPS alloy material provided by the present invention is prepared by adding hollow glass microspheres within a specific average particle size range, selecting ASA rubber powder within a specific acrylate mass content range, and matching other components in appropriate mass proportions. The obtained product can meet the halogen-free 5VA flame retardant grade when prepared into a thin-walled product (thickness ≤ 2 mm), and the 5VA flame retardant grade is achieved without adding an anti-dripping agent. At the same time, the obtained product has good toughness and rigidity.
[0009] Specifically, the addition of ASA rubber powder within a specific range of acrylic ester mass content can give full play to its polar and non-polar coexistence characteristics, play a bridging role between the polar hollow glass microsphere surface and the non-polar HIPS resin, effectively enhance the bonding force between the two, and improve the melt strength of the material, thereby improving the flame retardant and mechanical properties of the product. The addition of hollow glass microspheres within a specific average particle size range can not only play a role in heat insulation and slow down the speed of heat transfer, but also play a role in network nodes, enhance the melt strength of the material, prevent the material from being burned through, and further help improve the flame retardant and mechanical properties of the product; and hollow glass microspheres are low-density materials, which as a component of HIPS alloy materials can reduce the density of HIPS alloy materials, thereby reducing production costs. In addition, the addition of a compatibilizer within a specific mass range can effectively improve the compatibility of HIPS and ASA rubber powder, thereby improving the overall compatibility of the system and improving the overall effect of the product.
[0010] The mass content of acrylate in the ASA rubber powder is calculated by gas chromatography. The method is based on the separation characteristics of acrylate in a gas chromatographic column, and utilizes the volatility of acrylate in the sample to perform quantitative analysis through the detector of a gas chromatograph. The specific steps are as follows: First, prepare the sample. Dissolve the sample to be tested in a suitable solvent to prepare a sample solution of a certain concentration. At the same time, add an internal standard for correction during quantitative analysis. Then, inject the sample into a gas chromatograph for testing, and perform quantitative analysis based on the results.
[0011] The average particle size of the hollow glass microspheres is obtained by testing with a laser particle size analyzer.
[0012] Exemplarily, the mass percentage of the polyamide resin can be any point value or any two point range values between 58-82 parts, such as 60-80 parts, or 58 parts, 60 parts, 62 parts, 64 parts, 66 parts, 68 parts, 70 parts, 72 parts, 74 parts, 76 parts, 78 parts, 80 parts, 82 parts, etc.; the ASA rubber powder can be any point value or any two point range values between 18-42 parts, such as 20-40 parts, or 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, etc.; the phosphorus-based flame retardant can be any point value or any two point range values between 10-18 parts, such as 12-16 parts, Or it can be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, etc.; the nitrogen-based flame retardant can be any point value or any two-point range value between 3-9 parts, for example, it can be 5-7 parts, or it can be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, etc.; the hollow glass microspheres can be any point value or any two-point range value between 4-12 parts, for example, it can be 6-10 parts, or it can be 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, etc.; the compatibilizer can be any point value or any two-point range value between 1-9 parts, for example, it can be 3-7 parts, or it can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, etc.
[0013] Exemplarily, in the ASA rubber powder, the mass content of acrylate can be any point value or any two point range values between 53-66%, for example, it can be 55-64%, or it can be 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, etc.
[0014] Exemplarily, the average particle size of the hollow glass microspheres can be any point value or any two point range values between 38-82μm, for example, 40-80μm, or 38μm, 40μm, 42μm, 45μm, 48μm, 50μm, 52μm, 55μm, 58μm, 60μm, 62μm, 65μm, 68μm, 70μm, 72μm, 75μm, 78μm, 80μm, 82μm, etc.
[0015] Preferably, the mass content of acrylate in the ASA rubber powder is 56-60%.
[0016] Preferably, the average particle size of the hollow glass microspheres is 55-65 μm.
[0017] Preferably, in the HIPS alloy material, the mass percentage of ASA rubber powder is 12-38%, and the mass percentage of hollow glass microspheres is 2-12%.
[0018] As a preferred embodiment of the HIPS alloy material of the present invention, the HIPS alloy material comprises the following components in parts by weight: 25-32 parts of ASA rubber powder, 8-9 parts of hollow glass microspheres, and 5-6 parts of a compatibilizer.
[0019] The present invention has found that the added amounts of ASA rubber powder, hollow glass microspheres and compatibilizer will affect the performance of the product. When the mass amounts of the three are further selected to be within the above range, the comprehensive performance of the obtained product is better.
[0020] As a preferred embodiment of the HIPS alloy material of the present invention, the rubber mass content of the HIPS resin is 15-28%.
[0021] Specifically, the rubber mass content of HIPS resin refers to the mass content of butadiene, and the rubber mass content of HIPS resin is obtained by solvent extraction test, which is as follows: First, the HIPS sample is fully mixed with an appropriate solvent (such as benzene, xylene, etc.) to dissolve the butadiene rubber in the solvent to form a solution. Then, by evaporating the solvent, a rubber residue is obtained. Finally, the mass of the rubber residue is compared with the mass of the initial HIPS sample to obtain the rubber content.
[0022] Exemplarily, the rubber mass content of the HIPS resin can be any point value or any two point range values between 15-28%, such as 18-25%, or 15%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 28%, etc.
[0023] Preferably, the rubber mass content of the HIPS resin may be 20-22%.
[0024] The present invention has found that the rubber mass content of HIPS resin affects the mechanical properties of the product and also has a certain influence on the flame retardant properties of the product. When the rubber mass content of HIPS resin is further selected to be 15-28%, especially 20-22%, the comprehensive effect of the obtained product is better.
[0025] As a preferred embodiment of the HIPS alloy material of the present invention, the compatibilizer includes at least one of styrene-maleic anhydride copolymer, maleic anhydride grafted SEBS, silicone, and maleic anhydride grafted ABS.
[0026] Preferably, the compatibilizer includes at least one of styrene-maleic anhydride copolymer and maleic anhydride grafted SEBS.
[0027] The present invention has found that the selection of a compatibilizer affects the compatibility between components, thereby affecting the melt strength of the product, and further affecting the overall performance of the product. When the compatibilizer is further selected as a substance of the above category, the overall performance of the obtained product is better.
[0028] As a preferred embodiment of the HIPS alloy material of the present invention, the phosphorus-based flame retardant includes at least one of bisphenol A-bis(diphenyl phosphate) and triphenyl phosphate.
[0029] As a preferred embodiment of the HIPS alloy material of the present invention, the nitrogen-based flame retardant includes at least one of melamine cyanurate and dicyandiamide.
[0030] As a preferred embodiment of the HIPS alloy material of the present invention, the HIPS alloy material further comprises 0.1-1 parts of a processing aid.
[0031] Preferably, the processing aid includes at least one of an antioxidant and a lubricant.
[0032] Exemplarily, the antioxidant includes at least one of a hindered phenol antioxidant, a hindered amine antioxidant, and a phosphite antioxidant.
[0033] Exemplarily, the lubricant includes at least one of a stearic acid amide lubricant and a zinc stearate lubricant.
[0034] In the second aspect of the present invention, the present invention also provides a method for preparing the HIPS alloy material, which comprises the following steps: weighing the dried raw materials, mixing them and sending them into a twin-screw extruder, extruding, drawing, cooling, pelletizing and drying to obtain the HIPS alloy material.
[0035] As a preferred embodiment of the preparation method of the present invention, the parameters of the twin-screw extruder are: the aspect ratio of the twin-screw extruder is (40-36):1, the screw speed is 250-300rpm, and the extrusion temperature is 190-200°C.
[0036] In the third aspect of the present invention, the present invention also provides the use of the HIPS alloy material in preparing flame-retardant ultra-thin materials.
[0037] For example, HIPS alloy materials are used in the preparation of various household appliance housings, printer panels, automobile interiors and other materials.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] A HIPS alloy material provided by the present invention is prepared by adding hollow glass microspheres within a specific average particle size range, selecting ASA rubber powder within a specific acrylic ester mass content range, and matching other components in appropriate mass parts. The obtained product can meet the halogen-free 5VA flame retardant grade when prepared into a thin-walled product (thickness ≤ 2 mm) without adding an anti-dripping agent, and the obtained product has good toughness and strength; specifically, the Izod notched impact strength of the obtained HIPS alloy material is 18.3 kJ / m 2 The above-mentioned properties have a bending strength of more than 27.5 MPa and a flame retardant property that meets the 2.0 mm 5VA grade. In addition, the preparation method of the HIPS alloy material provided by the present invention is simple and is conducive to actual production. DETAILED DESCRIPTION
[0040] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0041] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0042] HIPS-1: PS1180, rubber content 21.4wt%, Trinseo, USA;
[0043] HIPS-2: PS HI-425TVL, rubber content 18.1wt%, Kumho Petrochemical Co., Ltd., South Korea;
[0044] HIPS-3: PS PH-888G, rubber content 25.0wt%, Chi Mei Chemical Co., Ltd., Taiwan;
[0045] HIPS-4: PS 514P, rubber content 15.3wt%, Shanghai Secco Petrochemical Co., Ltd.
[0046] HIPS-5: PS1110, rubber content 27.2wt%, Trinseo, USA;
[0047] ASA rubber powder 1: M800, acrylate content 58w.t.%, Zhejiang Suqi New Materials Co., Ltd.;
[0048] ASA rubber powder 2: A600N, acrylate content 55w.t.%, Zhejiang Changhong Plastic Raw Materials Co., Ltd.;
[0049] ASA rubber powder 3: Q350KL, acrylate content 64w.t.%, Zhejiang Suqi New Materials Co., Ltd.;
[0050] ASA rubber powder 4: XC-500A, acrylate content 50w.t.%, Kumho Petrochemical Co., Ltd., South Korea;
[0051] ASA rubber powder 5: EM500, acrylate content 70w.t.%, Dongguan Huiyi Chemical Materials Co., Ltd.;
[0052] Hollow glass microspheres 1: HN20, average particle size 60 μm, Shanxi Hainuo Technology Co., Ltd.
[0053] Hollow glass microsphere 2: 320#, average particle size 40 μm, Lingshou Baiyi Mineral Products Company;
[0054] Hollow glass microsphere 3: 220#, average particle size 80μm, Lingshou Baiyi Mineral Products Company;
[0055] Hollow glass microsphere 4: HN16K, average particle size 30 μm, Shanxi Hainuo Technology Co., Ltd.
[0056] Hollow glass microspheres 5: 180#, average particle size 90μm, Lingshou Baiyi Mineral Products Company;
[0057] Solid glass beads 6: 220 mesh glass beads, average particle size 50 μm, Okey Mineral Products Company;
[0058] Compatibilizer 1: SEBS FG1901 GT, maleic anhydride grafted SEBS, Kraton, USA;
[0059] Compatibilizer 2: SMA700, styrene-maleic anhydride copolymer, Shanghai Huawen Electronic New Materials Co., Ltd.;
[0060] Compatibilizer 3: KT-2, maleic anhydride grafted ABS, Shenyang Ketong Plastic Technology Co., Ltd.;
[0061] Compatibilizer 4: MB50-002, silicone, Dow Corning;
[0062] Phosphorus flame retardant: bisphenol A-bis(diphenyl phosphate), commercially available;
[0063] Nitrogen flame retardant: melamine cyanurate, commercially available;
[0064] Antioxidant: Hindered amine antioxidant, commercially available;
[0065] Lubricant: Stearic acid amide lubricant, commercially available.
[0066] The antioxidants and lubricants used in the parallel experiments of the embodiments and comparative examples were consistent.
[0067] Examples 1-16 and Comparative Examples 1-9
[0068] The embodiments and comparative examples of the present invention provide a HIPS alloy material, and the component contents (parts by weight) of the HIPS alloy material are shown in Tables 1-3;
[0069] Table 1
[0070]
[0071] Table 2
[0072] Example 10 Embodiment 11 Example 12 Embodiment 13 Embodiment 14 Embodiment 15 Example 16 HIPS-1 70 70 70 70 70 70 70 ASA Rubber Powder 1 / / 25 25 25 25 25 ASA Rubber Powder 2 25 / / / / / / ASA Rubber Powder 3 25 / / / / / Phosphorus flame retardants 14 14 14 14 14 14 14 Nitrogen flame retardant 6 6 6 6 6 6 6 Hollow glass microspheres1 8 8 / 8 8 8 Hollow glass microspheres 2 / / 8 / / / / Hollow glass microspheres 3 / / / 8 / / / Compatibilizer 1 5 5 5 5 / / / Compatibilizer 2 / / / / 5 / / Compatibilizer 3 / / / / / 5 / Compatibilizer 4 / / / / / / 5
[0073] Table 3
[0074]
[0075] The preparation method of the HIPS alloy material provided in Example 1 is:
[0076] The dried raw materials are weighed, mixed and fed into a twin-screw extruder, and subjected to extrusion, strand drawing, cooling, pelletizing and drying to obtain a HIPS alloy material;
[0077] The parameters of the twin-screw extruder are as follows: the aspect ratio of the twin-screw extruder is 40:1, the screw speed is 280 rpm, and the extrusion temperature is 195°C.
[0078] The preparation methods of the HIPS alloy materials provided in Examples 2-16 and Comparative Examples 1-9 are consistent with that in Example 1, except that no relevant components are added.
[0079] Effect example
[0080] The effect examples of the present invention verify the performance of the products prepared in the embodiments and comparative examples; the test items include the following aspects:
[0081] 1. Bending strength test: The test standard refers to "ISO 178-2010 Determination of flexural properties of plastics";
[0082] 2. Izod notch impact strength test: The test standard refers to "ISO 180-2000 Determination of IZOD impact strength of plastics", and the notch type is type A;
[0083] 3. 5VA flame retardancy test: the test standard refers to "UL 94-2018 Flammability Test for Equipment and Appliance Component Materials", sample thickness 1.5 / 2.0mm;
[0084] The test results are shown in Table 4;
[0085] Table 4
[0086]
[0087] It can be seen from Table 4 that when the technical solution of the present invention is adopted, the obtained product has excellent mechanical properties and flame retardant properties; specifically, the Izod notched impact strength of the obtained product is 18.3 kJ / m 2 Above, the bending strength is above 27.5MPa, and they all have 2.0mm 5VA flame retardant grade;
[0088] It can be seen from Examples 1-4 and Comparative Examples 1-3 that the quality of the components has a great influence on the comprehensive performance of the product. When the mass parts of the components in Comparative Examples 1-3 are not within the range given in the present invention, the flame retardant performance of the obtained products is significantly reduced and cannot meet the 2.0mm 5VA flame retardant grade; and when the mass parts of the components are further selected to be within the preferred range of the present invention, the obtained products can meet the 1.5mm 5VA flame retardant grade;
[0089] It can be seen from Example 1, Examples 10-11 and Comparative Examples 8-9 that the mass content of acrylate in the ASA rubber powder will also affect the performance of the product. When the mass content of acrylate in the ASA rubber powder in Comparative Examples 8-9 is not within the given range, the obtained product cannot meet the thin-wall (thickness ≤ 2.00 mm) 5VA flame retardant grade;
[0090] It can be seen from Example 1, Examples 12-13 and Comparative Examples 5-6 that the average particle size of the hollow glass microspheres will also affect the flame retardant properties of the product. When the average particle size of the hollow glass microspheres in Comparative Examples 5-6 is not within the range given in the present invention, the obtained product cannot meet the thin-walled (thickness ≤ 2.00 mm) 5VA flame retardant grade; it can be seen from Example 1 and Comparative Example 4 that when the hollow glass microspheres are not added, the obtained product not only cannot meet the 5VA flame retardant grade, but also the bending strength shows a certain downward trend; it can be seen from Example 1 and Comparative Example 7 that when solid glass microspheres are used instead of hollow glass microspheres, the obtained product cannot meet the thin-walled (thickness ≤ 2.00 mm) 5VA flame retardant grade.
[0091] Finally, it should be noted that the above embodiments are intended to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A HIPS alloy material, characterized in that: The HIPS alloy material comprises the following components in parts by mass: 58-82 parts of HIPS resin, 18-42 parts of ASA rubber powder, 10-18 parts of phosphorus flame retardant, 3-9 parts of nitrogen flame retardant, 4-12 parts of hollow glass microspheres, 1-9 parts of compatibilizer; In the ASA rubber powder, the mass content of acrylate is 53-66%; The average particle size of the hollow glass microspheres is 38-82 μm.
2. The HIPS alloy material according to claim 1, characterized in that: The HIPS alloy material comprises the following components in parts by weight: 25-32 parts of ASA rubber powder, 8-9 parts of hollow glass microspheres, and 5-6 parts of a compatibilizer.
3. The HIPS alloy material according to claim 1, characterized in that: The rubber mass content of the HIPS resin is 15-28%.
4. The HIPS alloy material according to claim 1, characterized in that: The compatibilizer includes at least one of styrene-maleic anhydride copolymer, maleic anhydride grafted SEBS, silicone, and maleic anhydride grafted ABS.
5. The HIPS alloy material according to claim 1, characterized in that: The phosphorus-based flame retardant includes at least one of bisphenol A-bis(diphenyl phosphate) and triphenyl phosphate.
6. The HIPS alloy material according to claim 1, characterized in that: The nitrogen-based flame retardant includes at least one of melamine cyanurate and dicyandiamide.
7. The HIPS alloy material according to claim 1, characterized in that: The HIPS alloy material also includes 0.1-1 parts of processing aids.
8. The method for preparing the HIPS alloy material according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: weighing the dried raw materials, mixing them and sending them into a twin-screw extruder, extruding, drawing, cooling, pelletizing and drying to obtain a HIPS alloy material.
9. Use of the HIPS alloy material according to any one of claims 1 to 7 in the preparation of flame-retardant ultra-thin materials.
Citation Information
Patent Citations
Light halogen-free flame-retardant reinforced polyamide composition and preparation method thereof
CN108239394A
Flame-retardant HIPS (High Impact Polystyrene) material
CN113444335A
Air conditioner chassis and preparation method thereof
CN115895161A
Thermoplastic resin composition
JP1992126771A
Cited By
Hips alloy material, and preparation method therefor and use thereof
WO2026056833A1