PBSeT / lignin composite material and preparation method and application thereof
By adding lignin compounds to PBSeT and using epoxy functional group compatibilizers, the compatibility of materials is improved, and the mechanical properties and cost of existing degradable plastic materials are solved, and high tensile strength and elongation of break are achieved. The improvement and reduction of production costs are applicable to packaging materials and plastic films.
Patent Information
- Application Number
- CN202310659652.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-06
AI Technical Summary
Existing biodegradable plastic materials have shortcomings in terms of mechanical properties and costs, and the utilization rate of lignin is low, resulting in waste of resources and environmental pollution.
By adding lignin compounds to PBSeT and using a compatibilizer containing epoxy functional groups, the compatibility of the material is improved through chemical reactions and physical actions, thereby improving mechanical properties and reducing costs.
The high tensile strength and elongation of break of PBSeT/lignin composites have been achieved, reaching 18MPa and 1159%, while reducing production costs and are suitable for packaging materials and plastic films.
Smart Images

Figure CN119081360A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of degradable films and relates to a PBSeT / lignin composite material and a preparation method and application thereof. Background Art
[0002] While the use of plastics brings a lot of convenience to people, it also causes problems such as energy crisis and white pollution. The raw materials of degradable plastics come from crops. Under the action of compost, microorganisms, light, water vapor, etc., degradable plastics can be degraded into carbon dioxide and water. It is a green, recyclable and environmentally friendly material. The development of degradable plastics is an important way to solve these problems. PBSeT (polybutylene sebacic acid-terephthalate) is a degradable material with good toughness and processing properties.
[0003] Patent CN114456488A discloses a tear-resistant PBSeT / PP / HDPE composite material, which is to first melt blend PP and HDPE in the first stage, and then add the synthesized PBSeT to blend. When the PBSeT content is 12%, the elongation at break is 357.65%. Patent CN113396039A discloses a method for preparing a starch blend, which uses PBAT as the main resin, adds starch and other additives for melt blending, and then blows to obtain a film, wherein the maximum elongation at break can reach 539%. Patent CN103703077A discloses a biodegradable film, which uses PBAT and poly (3-hydroxybutyrate-co-3-hydroxyhexanoate) as the resin matrix, adds fillers and additives such as calcium carbonate talc, and performs melt extrusion blow molding, and the maximum elongation at break of the obtained degradable film can reach 907%.
[0004] Lignin is the second largest biomass resource in the plant kingdom after cellulose. In industry, lignin is a byproduct of pulping, papermaking and bioethanol production. It is a sustainable and inexpensive biomass material. However, the utilization rate of lignin is low. It is mostly discharged into rivers in the form of waste liquid or burned after concentration, resulting in huge waste of resources every year. Due to its own structural characteristics, lignin has the advantages of safety, non-toxicity, low cost, UV absorption, biodegradability, antibacterial and antioxidant properties, and has the potential to be used as a reinforcing filler for composite materials. Summary of the invention
[0005] The present invention provides a PBSeT / lignin composite material and a preparation method thereof, which improves the compatibility of PBSeT with lignin compounds, and synergistically improves the compatibility of PBSeT with lignin compounds through chemical reactions and physical effects between components, thereby achieving the purpose of improving the mechanical properties of the product and reducing costs. The composite material provided by the present invention has a high content of lignin compounds, is a completely degradable, environmentally friendly bioplastic with no pollution to the environment, and is suitable for packaging materials, ground films and other fields.
[0006] One of the objects of the present invention is to provide a PBSeT / lignin composite material, comprising a mixture of PBSeT, a lignin compound, a compatibilizer and / or a reaction product thereof, wherein the compatibilizer is selected from organic compounds containing epoxy functional groups.
[0007] According to the present invention, in the PBSeT / lignin composite material:
[0008] The lignin compound may be a commonly used lignin compound in the art, preferably at least one selected from alkali lignin, enzymatic lignin, and lignin sulfonate;
[0009] The compatibilizer is selected from at least one of epoxidized soybean oil and a copolymer containing epoxy functional groups; wherein the copolymer containing epoxy functional groups is preferably an acrylic acid and styrene copolymer containing epoxy functional groups, for example, commercially available products ADR-4468, ADR-4400, etc.
[0010] According to the present invention, the PBSeT / lignin composite material optionally further comprises at least one of a coupling agent and an opening agent, wherein the coupling agent is selected from at least one of silane coupling agents; the opening agent is selected from fatty amide compounds, preferably at least one of erucic acid amide and oleic acid amide; based on the total weight of the PBSeT and lignin compounds as 100 parts by weight, the coupling agent is 0 to 5 parts, and the opening agent is 0 to 1 part; preferably, based on the total weight of the PBSeT and lignin compounds as 100 parts by weight, the coupling agent is 0 to 3 parts, and the opening agent is 0.05 to 0.5 parts.
[0011] According to the present invention, in the PBSeT / lignin composite material, based on the total weight of the PBSeT and the lignin compound as 100 parts by weight, the PBSeT is 50 to 99 parts, the lignin compound is 1 to 50 parts, and the compatibilizer is 0.1 to 12 parts; preferably, the PBSeT is 70 to 90 parts, the lignin compound is 10 to 30 parts, and the compatibilizer is 1 to 10 parts.
[0012] The second object of the present invention is to provide a method for preparing the above-mentioned PBSeT / lignin composite material, comprising: premixing the components including the PBSeT, lignin compounds, and a compatibilizer, and then melt-extruding and granulating to obtain the PBSeT / lignin composite material.
[0013] According to the present invention, in the method for preparing the PBSeT / lignin composite material:
[0014] The PBSeT and lignin compounds need to be dried in advance. The drying process can be carried out using the drying equipment and drying conditions commonly used in the art. Preferably, the drying conditions are: drying at 60-70° C. for 20-24 hours;
[0015] At least one of a coupling agent and an opening agent is optionally added during the premixing process, wherein the coupling agent is selected from at least one of silane coupling agents; the opening agent is selected from fatty amide compounds, preferably at least one of erucamide and oleamide.
[0016] According to the present invention, in the preparation method of the PBSeT / lignin composite material, the melt extrusion can adopt the melt extrusion equipment and melt extrusion process commonly used in the art, preferably carried out on a twin-screw extruder, with a screw speed of 100 to 140 rpm; the melt extrusion temperature is 100 to 180°C, preferably 110 to 170°C.
[0017] According to a specific embodiment of the present invention, the preparation method of the PBSeT / lignin composite material can specifically adopt the following preparation process:
[0018] (1) Pretreatment of raw materials: 50-99 parts of PBSeT and 1-50 parts of lignin compounds are placed in a forced air drying oven and dried at a temperature of 60-70° C. for 20-24 hours to remove moisture from the raw materials;
[0019] (2) Mixing of raw materials: Add 50-99 parts of the dried PBSeT, 1-50 parts of lignin, 0.1-12 parts of a compatibilizer, 0-5 parts of a coupling agent, and 0-1 part of an opening agent into a high-speed mixer and mix them uniformly to obtain a premix. The speed is 1000-2000 r / min and the mixing time is 10-20 min.
[0020] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 35 to 45:1, a feeding speed of 10 to 14 rpm, a screw speed of 100 to 140 rpm, and the temperature of each zone is controlled at: 100 to 125°C for zone 1, 130 to 160°C for zone 2, 140 to 170°C for zone 3, 140 to 170°C for zone 4, 140 to 170°C for zone 5, 130 to 160°C for zone 6, and 130 to 160°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite material.
[0021] The present invention chemically reacts the epoxy functional group in the compatibilizer with the hydroxyl and / or carboxyl group in PBSeT and / or lignin compounds to perform reaction and compatibilization, thereby forming a PBSeT-compatibilizer-lignin microbranched structure. In the PBSeT / lignin composite material provided by the present invention, a coupling agent is optionally added according to actual application needs, and the compatibilization can be synergistically increased through the chemical reaction of the compatibilizer and the physical action of the coupling agent, thereby improving the compatibility of PBSeT and lignin compounds and improving the mechanical properties of the composite material.
[0022] The third object of the present invention is to provide a PBSeT-based biodegradable film, which is prepared from the above-mentioned PBSeT / lignin composite material or the PBSeT / lignin composite material obtained by the above-mentioned preparation method.
[0023] A fourth object of the present invention is to provide a method for preparing the above-mentioned PBSeT-based biodegradable film, comprising the step of extruding and casting the PBSeT / lignin composite material into a film.
[0024] According to the present invention, the extrusion casting can adopt the extrusion casting equipment and extrusion casting conditions commonly used in the art. Preferably, the extrusion casting conditions are: temperature of 100-180°C, preferably 110-170°C; screw speed of 40-80rpm; pulling rate of 0.1-2.5m / min.
[0025] According to a specific embodiment of the present invention, the preparation method of the PBSeT-based biodegradable film can specifically adopt the following preparation process:
[0026] Extrusion casting film: the masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 100-120°C for zone 1, 115-145°C for zone 2, 140-160°C for zone 3, 140-160°C for zone 4, 145-165°C for zone 5, 145-165°C for zone 6, 155-180°C for zone 7, and 155-180°C for zone 8, the screw speed is 40-80rpm, the pulling rate is 0.1-2.5m / min, and after cooling and curling, the PBSeT-based biodegradable film is obtained. The thickness of the obtained film is 30-150μm.
[0027] A fifth object of the present invention is to provide the use of the above-mentioned PBSeT / lignin composite material or the above-mentioned PBSeT-based biodegradable film in agricultural mulch films and packaging materials.
[0028] By adopting the above technical scheme, the PBSeT-based biodegradable film obtained by the present invention has good toughness and low cost, good processing performance, and the optimized performances of tensile strength and elongation at break can reach 18MPa and 1159% respectively.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. In the present invention, an organic compound containing an epoxy functional group is added as a compatibilizer to improve the compatibility between PBSeT and lignin compounds, thereby improving the mechanical properties of the composite material;
[0031] 2. The components in the composite material of the present invention are environmentally friendly materials. When the performance and cost of the composite material are comprehensively considered, the optimized performance of the tensile strength and elongation at break of the composite material can reach 18MPa and 1159% respectively;
[0032] 3. The preparation process provided by the present invention is simple and easy to implement, and can be easily industrialized and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figures 1-2 It is the infrared spectrum test graph of the PBSeT / lignin degradable composite film prepared in Example 1 of the present invention, and PBSeT, epoxidized soybean oil (ESO) and enzymatic lignin (Lignin). DETAILED DESCRIPTION
[0034] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0035] The test instruments and test conditions used in the examples are as follows:
[0036] The tensile properties of the PBSeT / lignin degradable composite film were measured using a universal testing machine (MTSE42.503) according to the national standard GB / T1040.3-2006.
[0037] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0038] Embodiment 1:
[0039] (1) Pretreatment of raw materials: 70 parts of PBSeT and 30 parts of enzymatically hydrolyzed lignin were placed in a forced air drying oven and dried at 70° C. for 20 h to remove moisture from the raw materials.
[0040] (2) Mixing of raw materials: 70 parts of the dried PBSeT, 30 parts of enzymatic lignin, 2 parts of epoxidized soybean oil, 0.5 parts of KH550 coupling agent, and 0.05 parts of erucamide were added into a high-speed mixer and mixed evenly to obtain a premix. The speed was 1600 r / min and the mixing time was 15 min.
[0041] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding rate of 12 rpm, a screw speed of 120 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0042] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C for zone 1, 135°C for zone 2, 155°C for zone 3, 155°C for zone 4, 160°C for zone 5, 160°C for zone 6, 170°C for zone 7, and 170°C for zone 8. The screw speed is 60rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 120μm. The tensile strength is 16MPa, and the elongation at break can reach 1097%.
[0043] The infrared characterization of the prepared PBSeT / lignin biodegradable composite film is shown in the attached figure. Figures 1-2 As shown in the figure, the hydroxyl group of lignin is at 3419cm -1 There is a broad stretching vibration peak at 823 cm-1.-1 and 724cm -1 It can be found that the absorption peaks of epoxy groups and hydroxyl groups in PBSeT / lignin disappeared, proving that the epoxy groups and hydroxyl groups reacted chemically to form a PBSeT-compatibilizer-lignin microbranched structure.
[0044] Embodiment 2:
[0045] (1) Pretreatment of raw materials: 70 parts of PBSeT and 30 parts of enzymatically hydrolyzed lignin were placed in a forced air drying oven and dried at 70° C. for 20 h to remove moisture from the raw materials.
[0046] (2) Mixing of raw materials: 70 parts of the dried PBSeT, 30 parts of enzymatic lignin, 2 parts of epoxidized soybean oil, 0 parts of KH560 coupling agent, and 0.05 parts of erucamide were added to a high-speed mixer and mixed evenly to obtain a premix. The speed was 1600 r / min and the mixing time was 15 min.
[0047] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding rate of 12 rpm, a screw speed of 120 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0048] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C for zone 1, 135°C for zone 2, 155°C for zone 3, 155°C for zone 4, 160°C for zone 5, 160°C for zone 6, 170°C for zone 7, and 170°C for zone 8. The screw speed is 60rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 90μm. The tensile strength is 13MPa, and the elongation at break can reach 1050%.
[0049] Embodiment 3:
[0050] (1) Pretreatment of raw materials: 70 parts of PBSeT and 30 parts of enzymatically hydrolyzed lignin were placed in a forced air drying oven and dried at 70° C. for 20 h to remove moisture from the raw materials.
[0051] (2) Mixing of raw materials: 70 parts of the dried PBSeT, 30 parts of enzymatic lignin, 1 part of epoxidized soybean oil, 1 part of KH550 coupling agent, and 0.05 parts of erucamide were added into a high-speed mixer and mixed evenly to obtain a premix. The speed was 1600 r / min and the mixing time was 15 min.
[0052] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding rate of 11 rpm, a screw speed of 110 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0053] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C for zone 1, 135°C for zone 2, 155°C for zone 3, 155°C for zone 4, 160°C for zone 5, 160°C for zone 6, 170°C for zone 7, and 170°C for zone 8. The screw speed is 60rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 73μm. It is measured that the tensile strength of the film is 15MPa, and the elongation at break can reach 1149%.
[0054] Embodiment 4:
[0055] (1) Pretreatment of raw materials: 70 parts of PBSeT and 30 parts of enzymatically hydrolyzed lignin were placed in a forced air drying oven and dried at 70° C. for 20 h to remove moisture from the raw materials.
[0056] (2) Mixing of raw materials: 70 parts of the dried PBSeT, 30 parts of enzymatic lignin, 4 parts of epoxidized soybean oil, 1 part of KH560 coupling agent, and 0.05 parts of erucamide were added to a high-speed mixer and mixed evenly to obtain a premix. The speed was 1600 r / min and the mixing time was 15 min.
[0057] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding rate of 11 rpm, a screw speed of 110 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0058] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C in zone 1, 135°C in zone 2, 155°C in zone 3, 155°C in zone 4, 160°C in zone 5, 160°C in zone 6, 170°C in zone 7, and 170°C in zone 8. The screw speed is 60rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 86μm. It is measured that the tensile strength of the film is 14MPa, and the elongation at break can reach 1187%.
[0059] Embodiment 5:
[0060] (1) Pretreatment of raw materials: 70 parts of PBSeT and 30 parts of enzymatically hydrolyzed lignin were placed in a forced air drying oven and dried at 70° C. for 20 h to remove moisture from the raw materials.
[0061] (2) Mixing of raw materials: 70 parts of the dried PBSeT, 30 parts of enzymatic lignin, 1 part of epoxidized soybean oil, 3 parts of KH550 coupling agent, and 0.05 parts of erucamide were added into a high-speed mixer and mixed evenly to obtain a premix. The speed was 1600 r / min and the mixing time was 15 min.
[0062] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding speed of 13 rpm, a screw speed of 130 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0063] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C for zone 1, 135°C for zone 2, 155°C for zone 3, 155°C for zone 4, 160°C for zone 5, 160°C for zone 6, 170°C for zone 7, and 170°C for zone 8. The screw speed is 60rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 102μm. It is measured that the tensile strength of the film is 13MPa, and the elongation at break can reach 1008%.
[0064] Embodiment 6:
[0065] (1) Pretreatment of raw materials: 70 parts of PBSeT and 30 parts of enzymatically hydrolyzed lignin were placed in a forced air drying oven and dried at 70° C. for 20 h to remove moisture from the raw materials.
[0066] (2) Mixing of raw materials: 70 parts of the dried PBSeT, 30 parts of enzymatic lignin, 2 parts of epoxidized soybean oil, 1 part of KH560 coupling agent, and 0.05 parts of erucamide were added into a high-speed mixer and mixed evenly to obtain a premix. The speed was 1600 r / min and the mixing time was 15 min.
[0067] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding rate of 12 rpm, a screw speed of 120 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0068] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C for zone 1, 135°C for zone 2, 155°C for zone 3, 155°C for zone 4, 160°C for zone 5, 160°C for zone 6, 170°C for zone 7, and 170°C for zone 8. The screw speed is 60rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 45μm. It is measured that the tensile strength of the film is 18MPa, and the elongation at break can reach 1159%.
[0069] Embodiment 7:
[0070] (1) Pretreatment of raw materials: 80 parts of PBSeT and 20 parts of enzymatically hydrolyzed lignin were placed in a forced air drying oven and dried at 70° C. for 20 h to remove moisture from the raw materials.
[0071] (2) Mixing of raw materials: 80 parts of the dried PBSeT, 20 parts of enzymatic lignin, 4 parts of ADR-4468 extender, 2 parts of KH570 coupling agent, and 0.1 part of oleamide were added into a high-speed mixer and mixed evenly to obtain a premix. The speed was 1600 r / min and the mixing time was 15 min.
[0072] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding rate of 11 rpm, a screw speed of 110 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0073] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C for zone 1, 135°C for zone 2, 155°C for zone 3, 155°C for zone 4, 160°C for zone 5, 160°C for zone 6, 170°C for zone 7, and 170°C for zone 8. The screw speed is 70rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 130μm. It is measured that the tensile strength of the film is 11MPa, and the elongation at break can reach 1092%.
[0074] Embodiment 8:
[0075] (1) Pretreatment of raw materials: 80 parts of PBSeT and 20 parts of alkali lignin were placed in a forced air drying oven and dried at 70° C. for 20 h to remove moisture from the raw materials.
[0076] (2) Mixing of raw materials: 80 parts of the dried PBSeT, 20 parts of alkali lignin, 1 part of ADR-4400 compatibilizer, 2 parts of KH570 coupling agent, and 0.1 part of oleic acid amide are added together into a high-speed mixer and mixed evenly to obtain a premix. The speed is 1600 r / min and the mixing time is 15 min.
[0077] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding rate of 12 rpm, a screw speed of 120 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0078] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C in zone 1, 135°C in zone 2, 155°C in zone 3, 155°C in zone 4, 160°C in zone 5, 160°C in zone 6, 170°C in zone 7, and 170°C in zone 8. The screw speed is 60rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 127μm. It is measured that the tensile strength of the film is 11MPa, and the elongation at break can reach 1124%.
[0079] Embodiment 9:
[0080] (1) Pretreatment of raw materials: 90 parts of PBSeT and 10 parts of alkali lignin were placed in a forced air drying oven and dried at 70°C for 20 hours to remove moisture from the raw materials.
[0081] (2) Mixing of raw materials: 90 parts of the dried PBSeT, 10 parts of alkali lignin, 2 parts of ADR-4468 compatibilizer, 1 part of KH590 coupling agent, and 0.1 part of oleamide were added to a high-speed mixer and mixed evenly to obtain a premix. The speed was 1600 r / min and the mixing time was 15 min.
[0082] (3) Extrusion granulation: The premix is added into a twin-screw extruder. The screws of the twin-screw extruder rotate in the same direction, with an aspect ratio of 40:1, a feeding rate of 12 rpm, a screw speed of 120 rpm, and the temperature of each zone is controlled at: 115°C for zone 1, 150°C for zone 2, 155°C for zone 3, 155°C for zone 4, 155°C for zone 5, 150°C for zone 6, and 145°C for zone 7. The materials are effectively melt-mixed by the shearing action of the twin-screw extruder and then extruded and granulated to obtain a PBSeT / lignin composite masterbatch.
[0083] (4) Extrusion casting: The PBSeT / lignin composite material masterbatch is placed in an extrusion casting machine, and the temperature of each zone is controlled at: 115°C in zone 1, 135°C in zone 2, 155°C in zone 3, 155°C in zone 4, 160°C in zone 5, 160°C in zone 6, 170°C in zone 7, and 170°C in zone 8. The screw speed is 60rpm, and the pulling rate is 0.75m / min. After cooling and curling, the PBSeT-based biodegradable film is obtained, and the thickness of the film is 125μm. It is measured that the tensile strength of the film is 12MPa, and the elongation at break can reach 1136%.
[0084] Comparative Example 1
[0085] This comparative example is a blend containing starch and PBAT disclosed in Chinese patent CN113396039A, wherein the maximum elongation at break of the disclosed example can reach 539%. The optimized tensile strength and elongation at break of the PBSeT / lignin composite material prepared in the above examples 1 to 10 of the present invention can reach 18MPa and 1159% respectively, and the elongation at break of the blend in comparative example 1 is much lower than that of the present invention.
[0086] Comparative Example 2
[0087] This comparative example is a tear-resistant PBSeT / PP / HDPE composite material disclosed in Chinese patent CN114456488A, in which the elongation at break of the prepared material is 357.65%, which is much lower than that of the above-mentioned embodiments 1 to 10 of the present invention. In addition, the PP and HDPE used are non-degradable materials, while the PBSeT and lignin selected in the present invention are both degradable.
[0088] Comparative Example 3
[0089] In Comparative Example 3, a PBSeT / lignin composite material without a compatibilizer and a coupling agent was prepared in the same manner as in Example 1, and the tensile strength and elongation at break were 11 MPa and 997%, respectively. Compared with the material without a compatibilizer, it was found that the PBSeT / lignin composite material with a compatibilizer and a coupling agent added in Example 1 had better performance.
Claims
1. A PBSeT / lignin composite material, comprising a mixture of PBSeT, a lignin compound, a compatibilizer and / or a reaction product thereof, wherein the compatibilizer is selected from organic compounds containing epoxy functional groups.
2. The PBSeT / lignin composite material according to claim 1, characterized in that The lignin compound is selected from at least one of alkali lignin, enzymatic lignin and lignin sulfonate; and / or, The compatibilizer is selected from at least one of epoxidized soybean oil and a copolymer containing epoxy functional groups; and / or, The PBSeT / lignin composite material may optionally further comprise at least one of a coupling agent and an opening agent.
3. The PBSeT / lignin composite material according to claim 2, characterized in that The coupling agent is selected from at least one of silane coupling agents; and / or, The opening agent is selected from fatty amide compounds, preferably at least one of erucamide and oleamide; and / or, Based on the total weight of the PBSeT and the lignin compound as 100 parts by weight, the coupling agent is 0-5 parts, and the opening agent is 0-1 part; preferably, based on the total weight of the PBSeT and the lignin compound as 100 parts by weight, the coupling agent is 0-3 parts, and the opening agent is 0.05-0.5 parts.
4. The PBSeT / lignin composite material according to claim 1, characterized in that Based on the total weight of the PBSeT and the lignin compound as 100 parts by weight, the PBSeT is 50-99 parts, the lignin compound is 1-50 parts, and the compatibilizer is 0.1-12 parts; preferably, the PBSeT is 70-90 parts, the lignin compound is 10-30 parts, and the compatibilizer is 1-10 parts.
5. A method for preparing the PBSeT / lignin composite material according to any one of claims 1 to 4, comprising: The components including the PBSeT, lignin compounds and a compatibilizer are premixed, melt-extruded and granulated to obtain the PBSeT / lignin composite material.
6. The preparation method according to claim 5, characterized in that: The PBSeT and lignin compounds need to be dried in advance, preferably at 60-70° C. for 20-24 hours; and / or, At least one of a coupling agent and an opening agent is optionally added during the premixing process.
7. The preparation method according to claim 5, characterized in that: The melt extrusion is carried out on a twin-screw extruder, preferably, the screw speed is 100-140 rpm; and / or, The temperature of the melt extrusion is 100-180°C, preferably 110-170°C.
8. A PBSeT-based biodegradable film, prepared from the PBSeT / lignin composite material according to any one of claims 1 to 4 or the PBSeT / lignin composite material obtained by the preparation method according to any one of claims 5 to 7.
9. A method for preparing the PBSeT-based biodegradable film according to claim 8, comprising the step of extruding and casting the PBSeT / lignin composite material into a film.
10. The preparation method according to claim 9, characterized in that: The conditions of the extrusion casting are: The temperature is 100 to 180°C, preferably 110 to 170°C; and / or, The screw speed is 40 to 80 rpm; and / or, The pulling speed is 0.1~2.5m / min.
11. Use of the PBSeT / lignin composite material according to any one of claims 1 to 4 or the PBSeT-based biodegradable film according to claim 8 in agricultural mulch films and packaging materials.
Citation Information
Patent Citations
Biodegradable polyester film
CN103703077A
Method for preparing starch blends
CN113396039A
Tear-resistant PBSeT / PP / HDPE composite material and preparation method thereof
CN114456488A
PBAT composite film based on irradiation modification and preparation method thereof
CN105086383A
Completely-biodegradable film bag material and preparation method of film bag
CN109810476A