Hybrid coordination-driven thermoplastic aminated starch-based hot melt adhesive with high fluidity and matrix strength as well as preparation and application thereof

A thermoplastic aminated starch-based hot melt adhesive with hybrid coordination addresses the issues of low fluidity and matrix strength in traditional starch-based adhesives, achieving strong bonding to metals and other substrates with high fluidity and biodegradability.

CN119081601AActive Publication Date: 2024-12-06GUANGDONG TAIQIANG TECH IND CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411358356.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-06
Estimated Expiration
2044-09-27

AI Technical Summary

Technical Problem

Existing hot melt adhesives based on petroleum-based polymers face challenges with poor bonding to polar materials like metals due to low interfacial phase region thickness and are difficult to degrade naturally, while starch-based adhesives suffer from low fluidity and matrix strength.

Method used

A thermoplastic aminated starch-based hot melt adhesive is developed through hybrid coordination with acrylamide grafted starch, EVA resin, tackifier, and antioxidant, utilizing metal salts to form dynamic coordination bonds that enhance fluidity and matrix strength, allowing for improved bonding to metals and other substrates.

Benefits of technology

The adhesive achieves high metal bonding strength, with copper sheet lap bonding up to 6.1 MPa and aluminum strip peel strength up to 1227 N/m, while maintaining high-temperature fluidity and low-temperature adhesion, and is environmentally friendly with increased starch content and biodegradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081601A_ABST
    Figure CN119081601A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of hot melt adhesives, and discloses a hybrid coordination-driven thermoplastic aminated starch-based hot melt adhesive with high fluidity and matrix strength as well as a preparation method and application thereof. The thermoplastic aminated starch-based hot melt adhesive disclosed by the invention is prepared from the following components in parts by mass: 40 to 80 parts of hybrid coordination thermoplastic acrylamide grafted starch, 10 to 30 parts of ethylene-vinyl acetate copolymer, 10 to 30 parts of tackifier and 0.2 to 0.4 part of antioxidant. The hot melt adhesive prepared from the modified aminated starch is rich in amino groups, forms reinforced hydrogen bonds and coordination with an interface, has excellent bonding performance, not only has a good bonding effect on paper and non-woven fabrics, but also has relatively high metal bonding strength, the copper sheet lap bonding strength reaches 6.1 MPa, the aluminum strip peel strength reaches 1227 N / m, and the hot melt adhesive can be widely applied to the field of paper and non-woven fabrics. The material can be applied to the fields of vehicle interiors, furniture, food, packaging, papermaking, hygienic products and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hot melt adhesives, and in particular relates to a thermoplastic aminated starch-based hot melt adhesive with high fluidity and matrix strength driven by hybrid coordination, and a preparation method and application thereof. Background Art

[0002] Hot melt adhesive is an environmentally friendly, easy-to-use adhesive that is widely applicable to substrates. Currently, most commercial hot melt adhesives are mainly composed of petroleum-based polymers, such as ethylene-vinyl acetate copolymer (EVA resin), polyamide and polyurethane. The bonding properties of these materials mainly rely on covalent bonds. Due to the thickness of the interfacial phase region, the bonding effect with polar materials such as metals is poor. In addition, this type of traditional material is not easy to degrade naturally. With the increase in usage, hot melt adhesives face severe challenges in resource conservation and environmental protection.

[0003] As a common natural resource in nature, starch has the advantages of abundant sources, economy, and natural degradation, and is widely used in the preparation of hot melt adhesive materials. However, the cohesion of hot melt adhesives containing starch and the adhesion to the interface are usually based on forces such as hydrogen bonds, resulting in generally low hot melt adhesive matrix strength and bonding strength. In addition, raw starch usually needs to be used to prepare thermoplastic starch (TPS) by destroying its intermolecular hydrogen bonds and particle texture through plasticizers and shearing. Although TPS is thermoplastic, due to the rigid molecular chain structure of starch, it often exhibits low fluidity and permeability to the interface, making it difficult to achieve good adhesion to the bonding substrate.

[0004] CN114806463A modifies corn starch by a modifier and a composite plasticizer to improve the processing properties of thermoplastic starch and obtain a thermoplastic starch-based hot melt adhesive product. Ren et al. used self-modified thermoplastic starch and grafted PCL as the basic raw materials, cyclohexane oil as a plasticizer, hydrogenated petroleum resin or hydrogenated rosin resin as a tackifier, and heated and mixed to obtain a new type of thermoplastic starch hot melt adhesive. Patent CN440781 obtains modified starch through the steps of sodium hypochlorite oxidation, acrylamide polycondensation, and norbornane diisocyanate end group sealing treatment to obtain a hot melt adhesive with high bonding strength, good water resistance, and non-toxicity. However, the starch content in these starch-containing hot melt adhesives is usually not high, and it is impossible to simultaneously overcome the key problems of poor fluidity of hot melt adhesives at high temperatures and weak matrix strength at low temperatures. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a thermoplastic aminated starch-based hot melt adhesive with high fluidity and matrix strength driven by hybrid coordination.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned thermoplastic aminated starch-based hot melt adhesive.

[0007] Another object of the present invention is to provide an application of the above-mentioned thermoplastic aminated starch-based hot melt adhesive.

[0008] The purpose of the present invention is achieved through the following solutions:

[0009] A hybrid coordination driven thermoplastic aminated starch-based hot melt adhesive with high fluidity and matrix strength, comprising the following components in parts by weight: 40-80 parts of hybrid coordination thermoplastic acrylamide grafted starch, 10-30 parts of ethylene-vinyl acetate copolymer (EVA resin), 10-30 parts of tackifier, and 0.2-0.4 parts of antioxidant.

[0010] Furthermore, the viscosity of the tackifier is preferably 700-1800 cp (150° C.).

[0011] Furthermore, the tackifier may include at least one of rosin resin, hydrogenated rosin resin, etc., and more preferably includes rosin resin.

[0012] Furthermore, the antioxidant can be any conventional antioxidant in the art, such as antioxidant 168, antioxidant 1010, antioxidant 1076, etc., and more preferably includes antioxidant 1010.

[0013] Furthermore, the EVA resin is preferably EVA28400.

[0014] In the thermoplastic aminated starch-based hot melt adhesive of the present invention, the hybrid coordinated thermoplastic acrylamide grafted starch is prepared from the following components in parts by weight: 60-75 parts of aminated starch, 25-40 parts of plasticizer, 0.05-10 parts of metal salt, and 0.05-5 parts of organic acid.

[0015] Furthermore, the amine group grafting rate of the aminated starch is 5-50%, and more preferably includes a 10% grafting rate.

[0016] Furthermore, the aminated starch may include at least one of acrylamide grafted starch, triethylenetetramine starch, amine functionalized dialdehyde starch, etc., more preferably acrylamide grafted starch.

[0017] Furthermore, the plasticizer may be any plasticizer conventionally used in the art, such as at least one of glycerol, ethylene glycol, pentaerythritol, etc., more preferably glycerol.

[0018] Furthermore, the metal salt may include at least one of a soluble zinc salt, a soluble calcium salt, a soluble magnesium salt, and the like.

[0019] Furthermore, the soluble zinc salt may include at least one of zinc acetate, zinc chloride, zinc citrate, zinc tartrate and the like.

[0020] Furthermore, the soluble calcium salt may include at least one of calcium tartrate, calcium chloride, calcium acetate and the like.

[0021] Furthermore, the soluble magnesium salt may include magnesium chloride and the like.

[0022] Furthermore, the organic acid may include at least one of malic acid, tannic acid, citric acid, and succinic acid, more preferably malic acid.

[0023] In the thermoplastic aminated starch-based hot melt adhesive of the present invention, the hybrid coordinated thermoplastic acrylamide grafted starch is prepared by the following steps: aminated starch, plasticizer and metal salt are uniformly mixed in proportion, placed in an extruder for reaction extrusion molding, cooled and granulated to obtain the hybrid coordinated thermoplastic acrylamide grafted starch.

[0024] Furthermore, after being uniformly mixed, the material can be allowed to stand for 1-48 hours before extrusion granulation.

[0025] Furthermore, the extruder used may be a co-rotating parallel twin-screw extruder; the temperature from the feed port to the die of the extruder is 80-140° C., and the screw speed is 50-300 r / min, more preferably 120-150 r / min.

[0026] The hybrid coordination process of the hybrid coordinated thermoplastic acrylamide grafted starch of the invention has temperature-sensitive reversible characteristics.

[0027] The present invention uses aminated starch as a raw material, and first uses a plasticizer and a metal salt to modify it. Under the action of the plasticizer, metal ions, and high thermal shear field, the aminated starch unwinds, and further forms a mononuclear multi-tooth coordination bond with the metal ion through the amino group / hydroxyl group. Its role is that the coordination bond has dynamic characteristics, can be dissociated at high temperature and reorganized at low temperature, so that the thermoplastic aminated starch does not lose its hot processing fluidity while improving its matrix strength. Then, it is combined with EVA resin, tackifier, etc. to prepare a thermoplastic aminated starch-based hot melt adhesive. Compared with traditional thermoplastic starch-based hot melt adhesives, the hot melt adhesive prepared by using modified aminated starch in the present invention is rich in amino groups, can form reinforced hydrogen bonds and coordination with the interface, and has excellent bonding properties. And the thermoplastic aminated starch-based hot melt adhesive of the present invention not only has a good bonding effect on paper and non-woven fabrics, but also has a high metal bonding strength. The lap bonding strength of copper sheets can reach 6.1MPa, and the peeling strength of aluminum strips can reach 1227N / m.

[0028] The present invention also provides a method for preparing the above-mentioned thermoplastic aminated starch-based hot melt adhesive, comprising mixing the components in proportion and placing them in an internal mixer for melt blending, cooling and granulating to prepare the thermoplastic aminated starch-based hot melt adhesive.

[0029] Furthermore, the temperature of the internal mixer can be 120-170° C., the rotor speed can be 5-120 r / min, and the internal mixing time can be 5-60 min.

[0030] Furthermore, the temperature of the internal mixer can be 140-150° C., the rotor speed can be 80-120 r / min, and the internal mixing time can be 10-40 min.

[0031] The present invention also provides the application of the above-mentioned thermoplastic aminated starch-based hot melt adhesive. The thermoplastic aminated starch-based hot melt adhesive of the present invention exhibits excellent bonding effects on materials such as paper, non-woven fabrics, and metals, has high bonding strength, and can be used in the fields of vehicle interiors, furniture, food, packaging, papermaking, sanitary products, etc.

[0032] Compared with the prior art, the present invention has the following advantages:

[0033] (1) The thermoplastic aminated starch-based hot melt adhesive of the present invention not only has a good bonding effect on paper and non-woven fabrics, but also has a high metal bonding strength. The copper sheet lap bonding strength can reach 6.1 MPa, and the aluminum strip peel strength can reach 1227 N / m.

[0034] (2) Based on the excellent bonding performance of the thermoplastic aminated starch-based hot melt adhesive of the present invention to metal materials, adding fillers to its components can increase the strength of the colloid matrix without destroying the bonding strength with the metal, thereby further improving the bonding performance of the thermoplastic aminated starch-based hot melt adhesive to the metal matrix.

[0035] (3) The metal salt in the thermoplastic aminated starch-based hot melt adhesive component of the present invention, wherein the metal ions can promote the cleavage of glycosidic bonds during the thermoplastic processing, that is, have a degradative effect on the starch molecular chain, promote the decrease of starch molecular weight, broaden the molecular weight distribution, reduce the entanglement of molecular chains, and transform the originally rigid and brittle thermoplastic starch into a soft and sticky thermoplastic aminated starch. Through this transformation, the acid-modified TPS can be used as the main material of the hot melt adhesive (rather than a filler), which can not only provide a large number of hydroxyl groups to improve the adhesion to the bonding interface, but also eliminate the use of non-degradable viscosity regulators. In addition, the formation of a mononuclear multidentate coordination structure by metal ions and amine / hydroxyl groups can give the hot melt adhesive excellent high-temperature fluidity and low-temperature strong adhesion temperature-sensitive reversible dynamic properties.

[0036] (4) The thermoplastic aminated starch-based hot melt adhesive after hybrid coordination has better fluidity during high-temperature processing, and its proportion in the hot melt adhesive is greatly increased (up to 80wt% by mass), which can greatly reduce the use of petroleum-based materials; the thermoplastic aminated starch-based hot melt adhesive of the present invention is prepared with aminated starch, glycerol, and rosin resin as main raw materials, and has good biodegradability; the hot melt adhesive is not only efficient in preparation process, but also can be reused, which is more environmentally friendly. The thermoplastic aminated starch-based hot melt adhesive prepared by the present invention can be used in a wide range of applications, such as bonding paper, non-woven fabrics, metals, etc., and can be used in transportation interiors, furniture, packaging, and other industries. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0038] Figure 1 It is a SEM picture of the thermoplastic aminated starch-based hot melt adhesive of the present invention.

[0039] Figure 2-Figure 3 The SEM images of the hot melt adhesives prepared in Comparative Example 1 and Comparative Example 2 are shown respectively. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited thereto. The materials involved in the following examples can be obtained from commercial channels unless otherwise specified. The methods described are conventional methods unless otherwise specified. The amount of each component is measured by mass volume, g, mL.

[0041] The EVA resin (brand name: EVA28400) used in the following examples was purchased from Shanghai Haiyu Chemical Co., Ltd.; the rosin resin was purchased from Jinan Fugang Chemical Co., Ltd., with a viscosity of 700-1800 cp (150° C.) and a softening point of 110-120° C.

[0042] Example 1

[0043] 70 parts by mass of acrylamide grafted starch, 30 parts by mass of glycerol, 3 parts by mass of zinc acetate and 1 part by mass of malic acid were added to a blender and mixed evenly. After standing for 24 hours, the mixture was added to a co-rotating twin-screw extruder for reactive extrusion. The temperature from the feed port of the extruder to the die was set to 90-140° C. (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 90° C., 110° C., 130° C., 135° C., 140° C., 140° C., 135° C. and 130° C., respectively), the screw speed was 150 r / min, and hybrid coordinated thermoplastic acrylamide starch particles were obtained after cooling and granulation.

[0044] 50 parts by mass of the hybrid coordinated thermoplastic acrylamide starch prepared above, 25 parts by mass of EVA resin, 25 parts by mass of rosin resin, and 0.4 parts by mass of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 150° C. and the rotor speed was 80 r / min. After internal mixing for 10 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic acrylamide starch-based hot melt adhesive.

[0045] Example 2

[0046] 70 parts by mass of acrylamide grafted starch, 30 parts by mass of glycerol, 3 parts by mass of zinc acetate and 1 part by mass of malic acid were added to a blender and mixed evenly. After standing for 24 hours, the mixture was added to a co-rotating twin-screw extruder for reactive extrusion. The temperature from the feed port of the extruder to the die was set to 90-140° C. (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 90° C., 110° C., 130° C., 135° C., 140° C., 140° C., 135° C. and 130° C., respectively), the screw speed was 150 r / min, and hybrid coordinated thermoplastic acrylamide starch particles were obtained after cooling and granulation.

[0047] 60 parts by mass of hybrid coordinated thermoplastic acrylamide starch, 20 parts by mass of EVA resin, 20 parts by mass of rosin resin, and 0.4 parts by mass of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 150° C. and the rotor speed was 90 r / min. After internal mixing for 20 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic acrylamide starch-based hot melt adhesive.

[0048] Example 3

[0049] 70 parts by mass of acrylamide grafted starch, 30 parts by mass of glycerol, 3 parts by mass of zinc acetate and 1 part by mass of malic acid were added to a blender and mixed evenly. After standing for 24 hours, the mixture was added to a co-rotating twin-screw extruder for reactive extrusion. The temperature from the feed port of the extruder to the die was set to 90-140° C. (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 90° C., 110° C., 130° C., 135° C., 140° C., 140° C., 135° C. and 130° C., respectively), the screw speed was 150 r / min, and hybrid coordinated thermoplastic acrylamide starch particles were obtained after cooling and granulation.

[0050] 70 parts by mass of hybrid coordinated thermoplastic acrylamide starch, 15 parts by mass of EVA resin, 15 parts by mass of rosin resin, and 0.4 parts by mass of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 150° C. and the rotor speed was 100 r / min. After internal mixing for 30 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic acrylamide starch-based hot melt adhesive.

[0051] Example 4

[0052] 70 parts by mass of acrylamide grafted starch, 30 parts by mass of glycerol, 3 parts by mass of zinc acetate and 1 part by mass of malic acid were added to a blender and mixed evenly. After standing for 24 hours, the mixture was added to a co-rotating twin-screw extruder for reactive extrusion. The temperature from the feed port of the extruder to the die was set to 90-140° C. (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 90° C., 110° C., 130° C., 135° C., 140° C., 140° C., 135° C. and 130° C., respectively), the screw speed was 150 r / min, and hybrid coordinated thermoplastic acrylamide starch particles were obtained after cooling and granulation.

[0053] 80 parts by mass of hybrid coordinated thermoplastic acrylamide starch, 10 parts by mass of EVA resin, 10 parts by mass of rosin resin, and 0.4 parts by mass of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 150° C. and the rotor speed was 110 r / min. After internal mixing for 40 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic acrylamide starch-based hot melt adhesive.

[0054] Example 5

[0055] 70 parts by mass of triethylenetetramine starch, 30 parts by mass of glycerol, 3 parts by mass of zinc acetate and 1 part by mass of malic acid were added to a blender and mixed evenly. After standing for 24 hours, the mixture was added to a co-rotating twin-screw extruder for reactive extrusion. The temperature from the feed port of the extruder to the die was set to 90-140°C (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 90°C, 110°C, 130°C, 135°C, 140°C, 140°C, 135°C and 130°C, respectively), the screw speed was 150 r / min, and hybrid coordinated thermoplastic triethylenetetramine starch particles were obtained after cooling and granulation.

[0056] 80 parts by mass of hybrid coordinated thermoplastic triethylenetetramine starch, 10 parts by mass of EVA resin, 10 parts by mass of rosin resin and 0.4 parts by mass of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 140°C and the rotor speed was 120 r / min. After internal mixing for 40 minutes, the material was discharged, cooled and granulated to obtain a thermoplastic triethylenetetramine-based hot melt adhesive.

[0057] Example 6

[0058] 70 parts by mass of amino-functionalized dialdehyde starch, 30 parts by mass of glycerol, 3 parts by mass of zinc acetate, and 1 part by mass of malic acid were added to a blender and mixed evenly. After standing for 24 hours, the mixture was added to a co-rotating twin-screw extruder for reactive extrusion. The temperature from the feed port of the extruder to the die was set to 80-130°C (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 80°C, 100°C, 120°C, 125°C, 130°C, 130°C, 125°C, and 120°C, respectively), the screw speed was 120 r / min, and hybrid coordinated thermoplastic amino-functionalized dialdehyde starch particles were obtained after cooling and granulation.

[0059] 80 parts by mass of hybrid coordinated thermoplastic amine-functionalized dialdehyde starch, 10 parts by mass of EVA resin, 10 parts by mass of rosin resin, and 0.4 parts by mass of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 140°C and the rotor speed was 120 r / min. After internal mixing for 40 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic amine-functionalized dialdehyde starch-based hot melt adhesive.

[0060] Example 7

[0061] 60 parts by mass of acrylamide grafted starch, 40 parts by mass of glycerol, 3 parts by mass of zinc acetate and 1 part by mass of malic acid were added into a blender and mixed evenly. After standing for 24 hours, the mixture was added into a co-rotating twin-screw extruder for reaction extrusion. The temperature from the feed port of the extruder to the die was set to 80-120° C. (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 80° C., 90° C., 110° C., 115° C., 120° C., 120° C., 115° C. and 110° C., respectively), the screw speed was 120 r / min, and hybrid coordinated thermoplastic acrylamide grafted starch particles were obtained after cooling and granulation.

[0062] 80 parts by weight of hybrid coordinated thermoplastic acrylamide grafted starch, 10 parts by weight of EVA resin, 10 parts by weight of rosin resin, and 0.4 parts by weight of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 140° C. and the rotor speed was 120 r / min. After internal mixing for 40 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic acrylamide grafted starch-based hot melt adhesive.

[0063] Example 8

[0064] 75 parts by mass of acrylamide grafted starch, 25 parts by mass of glycerol, 3 parts by mass of zinc acetate and 1 part by mass of malic acid were added into a blender and mixed evenly. After standing for 24 hours, the mixture was added into a co-rotating twin-screw extruder for reaction extrusion. The temperature from the feed port of the extruder to the die was set to 90-140° C. (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 90° C., 110° C., 130° C., 135° C., 140° C., 140° C., 135° C. and 130° C., respectively), the screw speed was 120 r / min, and hybrid coordinated thermoplastic acrylamide grafted starch particles were obtained after cooling and granulation.

[0065] 80 parts by weight of hybrid coordinated thermoplastic acrylamide grafted starch, 10 parts by weight of EVA resin, 10 parts by weight of rosin resin, and 0.4 parts by weight of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 150° C. and the rotor speed was 120 r / min. After internal mixing for 40 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic acrylamide grafted starch-based hot melt adhesive.

[0066] Example 9

[0067] 70 parts by mass of acrylamide grafted starch, 30 parts by mass of glycerol, 4 parts by mass of calcium acetate and 1 part by mass of malic acid were added into a blender and mixed evenly. After standing for 24 hours, the mixture was added into a co-rotating twin-screw extruder for reaction extrusion. The temperature from the feed port of the extruder to the die was set to 80-130° C. (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 80° C., 100° C., 120° C., 125° C., 130° C., 130° C., 125° C. and 120° C., respectively), the screw speed was 120 r / min, and hybrid coordinated thermoplastic acrylamide grafted starch was obtained after cooling and granulation.

[0068] 80 parts by weight of hybrid coordinated thermoplastic acrylamide grafted starch, 10 parts by weight of EVA resin, 10 parts by weight of rosin resin, and 0.4 parts by weight of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 150° C. and the rotor speed was 120 r / min. After internal mixing for 40 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic acrylamide grafted starch-based hot melt adhesive.

[0069] Comparative Example 1

[0070] 70 parts by mass of ordinary corn starch, 30 parts by mass of glycerol and 1 part by mass of malic acid were added to a blender and mixed evenly. After standing for 24 hours, the mixture was added to a co-rotating twin-screw extruder for reactive extrusion. The temperature from the feed port of the extruder to the die was set to 80-130°C (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 80°C, 100°C, 120°C, 125°C, 130°C, 130°C, 125°C and 120°C, respectively), the screw speed was 120 r / min, and thermoplastic starch was obtained after cooling and granulation.

[0071] 60 parts by mass of thermoplastic starch, 20 parts by mass of EVA resin, 20 parts by mass of rosin resin, and 0.4 parts by mass of antioxidant 1010 were premixed uniformly by mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 150°C and the rotor speed was 120 r / min. After internal mixing for 40 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic starch-based hot melt adhesive.

[0072] Comparative Example 2

[0073] 70 parts by weight of acrylamide grafted starch corn starch, 30 parts by weight of glycerol and 1 part by weight of malic acid were added to a blender and mixed evenly. After standing for 24 hours, the mixture was added to a co-rotating twin-screw extruder for reactive extrusion. The temperature from the feed port of the extruder to the die was set to 90-140° C. (the temperatures from the feed port of the extruder to each temperature control zone of the die were set to 90° C., 110° C., 130° C., 135° C., 140° C., 140° C., 135° C. and 130° C., respectively), the screw speed was 150 r / min, and after cooling and granulation, thermoplastic acrylamide grafted starch particles without hybrid coordination were obtained.

[0074] 80 parts by weight of thermoplastic acrylamide grafted starch without hybrid coordination, 20 parts by weight of EVA resin, 20 parts by weight of rosin resin, and 0.4 parts by weight of antioxidant 1010 were premixed uniformly with mechanical stirring and then added into an internal mixer for melt blending. The temperature of the internal mixer was 150° C. and the rotor speed was 110 r / min. After internal mixing for 40 minutes, the material was discharged, cooled, and granulated to obtain a thermoplastic acrylamide grafted starch-based hot melt adhesive without hybrid coordination.

[0075] The hot melt adhesives prepared in the above Examples 1-9 and Comparative Examples 1-2 were subjected to a copper sheet lap bonding strength test (tested in accordance with GB / T7124-2008 standard, with a tensile rate of 5 mm / min); an aluminum tape peel strength test (tested in accordance with GB / T2791-1995 standard, with a tensile rate of 200 mm / min), and the test results are shown in Table 1.

[0076] Table 1

[0077]

[0078] As can be seen from Table 1, the addition of the hybrid coordinated thermoplastic acrylamide grafted starch of the present invention significantly improves the bonding strength of the hot melt adhesive to the metal. Specifically, on the one hand, the addition of thermoplastic aminated starch significantly improves the bonding strength of the hot melt adhesive, and on the other hand, hybrid coordination is crucial to improving the matrix strength of the hot melt adhesive. The hot melt adhesive is bonded to the interface of the substrate through hydrogen bonding force after fully contacting the bonding substrate, so good wetting and abundant polar groups are conducive to improving the interfacial bonding strength. In addition, the cohesive energy density and molecular weight distribution of the colloid play a decisive role in the bonding strength. In the process of melt extrusion of thermoplastic aminated starch, the metal salt activates and breaks the glycosidic bonds in the starch chain through metal coordination, causing the molecular chain entanglement to decrease, the molecular weight to decrease, the molecular weight distribution to change from narrow to wide, and the thermoplastic starch to change from rigid to flexible. The increase in the number of small molecules can improve the fluidity of the thermoplastic starch, which is conducive to the infiltration of the hot melt adhesive to the bonding substrate, and the part with a large molecular weight maintains the matrix strength of the thermoplastic starch.

[0079] In addition, hybrid coordination has the characteristics of high-temperature dissociation and low-temperature reorganization. This feature not only meets the good fluidity of hot melt adhesive at high temperature, but also gives the hot melt adhesive the need for high cohesive energy density at low temperature. In addition, small molecule starch chains can increase their apparent molecular weight through hybrid coordination, which helps to improve the toughness and cohesive energy density of the hot melt adhesive matrix and avoid the cohesive failure problem caused by low molecular weight components. Aminated modification of starch chains can introduce amine-rich side chains, and promote strong interactions between starch chains through amine-hydroxyl strengthened hydrogen bonds. More importantly, flexible amine groups are easier to diffuse between adhesive matrices to form a strong adhesive interface layer, thereby improving the affinity and bonding strength between the hot melt adhesive and the adhesive matrix. Through the introduction of metal ions, the hot melt adhesive has metal-amine coordination and metal-hydroxyl coordination. The formed hybrid coordination reversible cross-linking network gives the thermoplastic aminated starch chain effective dissipation of external stress, which can significantly improve its matrix strength. Therefore, by aminated starch and introducing metal salt coordination, a thermoplastic aminated starch-based hot melt adhesive with high fluidity / matrix strength can be achieved through hybrid coordination.

[0080] Furthermore, the compatibility of the hot melt adhesive was observed using SEM. Figure 1 This is a SEM image of the hybrid coordinated thermoplastic acrylamide grafted starch-based hot melt adhesive of Example 4 of the present invention. Figure 2 and Figure 3 They are SEM images of ordinary thermoplastic starch-based hot melt adhesive without hybrid coordination and thermoplastic acrylamide graft-based hot melt adhesive without hybrid coordination prepared in Comparative Example 1 and Comparative Example 2, respectively.

[0081] As can be seen from the figure, the interface compatibility between the hybrid coordinated thermoplastic acrylamide grafted starch and the EVA resin and rosin resin in the hot melt adhesive of the present invention is better, which is manifested in that the phase domain of EVA / rosin resin in the hybrid coordinated thermoplastic acrylamide grafted starch matrix is ​​smaller and basically concentrated in the nanometer range. This feature will help reduce the bonding defects of the hybrid coordinated thermoplastic acrylamide grafted starch-based hot melt adhesive and improve its bonding uniformity and interface layer thickness. In comparison, Figure 2 and Figure 3 The EVA / rosin resin is basically dispersed in the non-hybridized thermoplastic starch / acrylamide grafted starch hot melt adhesive in the form of micron-sized phase domains. This phenomenon fully demonstrates that the hybridized coordinated thermoplastic aminated starch helps to significantly improve the dispersibility of EVA / rosin resin.

[0082] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A thermoplastic aminated starch-based hot melt adhesive with high fluidity and matrix strength driven by hybrid coordination, characterized in that The components include the following components in parts by weight: 40-80 parts of hybrid coordinated thermoplastic acrylamide grafted starch, 10-30 parts of ethylene-vinyl acetate copolymer, 10-30 parts of viscosity enhancer, and 0.2-0.4 parts of antioxidant.

2. The thermoplastic aminated starch-based hot melt adhesive according to claim 1, characterized in that: The tackifier includes at least one of rosin resin and hydrogenated rosin resin; the antioxidant includes at least one of antioxidant 168, antioxidant 1010, and antioxidant 1076.

3. The thermoplastic aminated starch-based hot melt adhesive according to any one of claims 1 to 2, characterized in that: The hybrid coordinated thermoplastic acrylamide grafted starch is prepared from the following components in parts by weight: 60-75 parts of aminated starch, 25-40 parts of plasticizer, 0.05-10 parts of metal salt and 0.05-5 parts of organic acid.

4. The thermoplastic aminated starch-based hot melt adhesive according to claim 3, characterized in that: The amine group grafting rate of the aminated starch is 5-50%.

5. The thermoplastic aminated starch-based hot melt adhesive according to claim 3, characterized in that: The aminated starch includes at least one of acrylamide grafted starch, triethylenetetramine starch, and amino-functionalized dialdehyde starch; the plasticizer includes at least one of glycerol, ethylene glycol, and pentaerythritol; the metal salt includes at least one of soluble zinc salt, soluble calcium salt, and soluble magnesium salt; and the organic acid includes at least one of malic acid, tannic acid, citric acid, and succinic acid.

6. The thermoplastic aminated starch-based hot melt adhesive according to claim 5, characterized in that: The soluble zinc salt includes at least one of zinc acetate, zinc chloride, zinc citrate and zinc tartrate; the soluble calcium salt includes at least one of calcium tartrate, calcium chloride and calcium acetate; and the soluble magnesium salt includes magnesium chloride.

7. The thermoplastic aminated starch-based hot melt adhesive according to claim 3, characterized in that: The hybrid coordinated thermoplastic acrylamide grafted starch is prepared by the following steps: aminated starch, plasticizer and metal salt are uniformly mixed in proportion, placed in an extruder for reaction extrusion molding, cooled and granulated to obtain the hybrid coordinated thermoplastic acrylamide grafted starch.

8. A method for preparing the thermoplastic aminated starch-based hot melt adhesive according to any one of claims 1 to 7, characterized in that The method comprises the steps of mixing the components in proportion, placing the components in an internal mixer for melting and blending, cooling and granulating to prepare a thermoplastic aminated starch-based hot melt adhesive.

9. The preparation method according to claim 8, characterized in that The temperature of the internal mixer is 120-170°C, the rotor speed is 5-120r / min, and the internal mixing time is 5-60min.

10. Application of the thermoplastic aminated starch-based hot melt adhesive according to any one of claims 1 to 7 in the fields of vehicle interiors, furniture, food, packaging, papermaking, and sanitary products.

Citation Information

Patent Citations

  • Preparation of low-cost hot-melt adhesive

    CN101280162A

  • Thermoplastic starch based on coordination effect as well as preparation method and application of thermoplastic starch

    CN110498950A

  • Biodegradable TPS-based hot melt adhesive with high metal bonding strength as well as preparation and application of TPS-based hot melt adhesive

    CN114381218A

  • Antibacterial TPS-based hot melt adhesive with high matrix strength as well as preparation method and application of antibacterial TPS-based hot melt adhesive

    CN117165218A

  • Polyvinyl alcohol-starch derivative composition and its use

    JP1994073259A