Adhesive for extra-high voltage transformer laminated paperboard as well as preparation method and application of adhesive

By using the adhesive of phenolic epoxy vinyl ester resin and methyl ethyl ketone peroxide solution, combined with the thermal curing process, the existing adhesives are solved incomplete curing and insufficient thermal deformation temperature in ultra-high voltage transformer laminated paperboard, and high performance is achieved The laminated cardboard product meets the use requirements of ultra-high voltage transformers.

CN119081611APending Publication Date: 2024-12-06GLEIHOW NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411199472.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The adhesive for laminated paperboard of existing ultra-high voltage transformers releases toxic substances during the production process, which is incompletely cured, affects product quality, and the thermal deformation temperature is not high, which cannot meet the use requirements of ultra-high voltage transformers.

Method used

Phenolic epoxy vinyl ester resin is used as resin glue, and methyl ethyl ketone peroxide solution is used as curing agent. The weight ratio is 100:1 to 3. The adhesive is prepared by a thermal curing process, and the bonding of laminated paperboard is carried out under specific conditions. .

Benefits of technology

It improves the heat resistance and chemical stability of the adhesive, meets the performance requirements of F-class electrical insulating materials, has high electrical strength and shrinkage, is suitable for large-scale production, and does not release toxic substances. The overall performance is better than that of imported products from abroad.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017475920000021
    Figure BDA0005017475920000021
  • Figure BDA0005017475920000071
    Figure BDA0005017475920000071
  • Figure FDA0005017475910000011
    Figure FDA0005017475910000011
Patent Text Reader

Abstract

The invention relates to an adhesive for an extra-high voltage transformer laminated paperboard as well as a preparation method and application of the adhesive. The adhesive consists of a resin adhesive and a curing agent, wherein the weight part ratio of the resin adhesive to the curing agent is 100: (1-3); the resin adhesive comprises the following components in parts by weight: 62-72 parts of phenolic epoxy vinyl ester resin; 0.5 to 3 parts of an anti-settling agent; 0.1 to 0.2 part of a wetting dispersant; 0 to 0.01 part of a defoaming agent; and 25-37 parts of an insulating filler. The invention also provides a preparation method and application of the adhesive for the extra-high voltage transformer laminated paperboard. According to the invention, the technical problem of adhesives for domestic extra-high voltage transformer laminated paperboards is solved, the adhesive prepared by the invention is applied to adhesion of paperboards in the field of extra-high voltage transformers, and the prepared laminated paperboard product has excellent insulativity, electrical strength, heat resistance and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and in particular relates to an adhesive for ultra-high voltage transformer laminated paperboard, and a preparation method and application thereof. Background Art

[0002] The UHV grid is known as the "power highway" for its long-distance, large-capacity, low-loss, and small land occupation characteristics. The UHV transformer uses the principle of electromagnetic induction to convert the AC voltage and current of one system into the voltage and current of another system, thus realizing the transmission of electric energy in the UHV grid.

[0003] Laminated paperboard is mainly used to make insulating parts in UHV transformers, such as pallet pressure plates, lead brackets, etc. Laminated paperboard is light in weight and has good insulation effect, which is the key to controlling equipment quality. Laminated paperboard for UHV transformers requires uniform density, and must not have cracking, bubbles, degumming, stratification, etc. The glue layer must not be carbonized during processing, and it can maintain stable performance for a long time in the UHV and high-temperature transformer oil environment. In order to meet the above requirements, the adhesive for UHV transformer laminated paperboard must have excellent insulation, electrical strength, heat resistance and transformer oil environmental stability, and the thickness of the adhesive film is controlled by roller coating and other processes to obtain laminated paperboard with uniform density.

[0004] In the prior art, the main components of adhesives for laminated paperboards are phenolic resin glue, unsaturated polyester resin glue, etc. Among them, phenolic resin glue contains a large amount of solvents, which not only releases toxic and harmful substances in the process of producing adhesives, which is harmful to the environment and human body, but also the adhesive film often has problems such as incomplete curing during use, which affects the product quality. Unsaturated polyester resin glue adopts a room temperature curing process, and the viscosity of the glue liquid will gradually increase, affecting the thickness of the glue coating. In addition, the thermal deformation temperature of unsaturated polyester resin glue is not high and the shrinkage is large. Therefore, the laminated paperboard product formed by the adhesive in the prior art after bonding the paperboard of the ultra-high voltage transformer is not good, and cannot meet the use requirements of the laminated paperboard of the ultra-high voltage transformer. Summary of the invention

[0005] The present invention makes up for the deficiencies of the prior art and provides an adhesive for ultra-high voltage transformer laminated paperboard, wherein the adhesive is composed of a resin adhesive and a curing agent, wherein the weight ratio of the resin adhesive to the curing agent is 100:1-3; and the resin adhesive has the following component contents in parts by weight:

[0006]

[0007] Preferably, the phenolic epoxy vinyl ester resin is prepared according to the following steps: according to weight parts, 374 to 440 parts of phenolic epoxy resin are put into a reaction kettle, stirred and heated to 80°C, then 0.1 parts of stabilizer and 2 parts of N,N-dimethylaniline are added, and then 172 parts of methacrylic acid are added dropwise to the reaction kettle within 2 hours. After the addition is completed, the temperature is raised to 110°C to obtain a reaction solution. When the acid value of the reaction solution is 13 to 15 mgKOH / g, the temperature is lowered to 80°C, and 274 to 300 parts of styrene are added to obtain the phenolic epoxy vinyl ester resin.

[0008] Preferably, the brand of the phenolic epoxy resin is at least one of NPPN-631, NPPN-638S, F-44, and F-51.

[0009] Preferably, the stabilizer is at least one of o-methylhydroquinone, tert-butylhydroquinone and 2,5-di-tert-butylhydroquinone.

[0010] Preferably, the anti-settling agent is at least one of organic bentonite, fumed silica, and polyamide wax.

[0011] Preferably, the insulating filler is at least one of talc powder, silica powder, mica powder and kaolin.

[0012] Preferably, the curing agent is a methyl ethyl ketone peroxide solution, and the active oxygen content of the methyl ethyl ketone peroxide solution is 9.1-10%.

[0013] Another object of the present invention is to provide a method for preparing the adhesive for the ultra-high voltage transformer laminated paperboard. The preparation method is as follows: put phenolic epoxy vinyl ester resin into a reaction kettle, add an anti-settling agent, a wetting dispersant, a defoaming agent and an insulating filler in sequence, stir for 30 to 60 minutes to obtain a resin glue, mix the resin glue and a curing agent evenly, let stand for 20 to 60 minutes to defoam, and obtain an adhesive, wherein the composition of the resin glue and the ratio of the resin glue to the curing agent are the same as the composition of the resin glue and the ratio of the resin glue to the curing agent.

[0014] Another object of the present invention is to provide an application of the above-mentioned adhesive in bonding ultra-high voltage transformer laminated paperboard, wherein the above-mentioned adhesive is evenly applied to the paperboard by single-sided coating, and then another paperboard is overlapped on the paperboard coated with the adhesive, and the number of times the above-mentioned operation is repeated is determined according to the number of layers of paperboard to be prepared, and then the neatly overlapped paperboard is sent to a hot pressing device, and maintained for 1 to 2 hours under the conditions of a unit pressure of 3 to 6 MPa and a temperature of 100 to 120° C., and then cooled to 40° C. and depressurized to normal pressure, so that the paperboard bonding is completed to obtain ultra-high voltage transformer laminated paperboard.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. The heat deformation temperature of the resin adhesive in the present invention is 165-170°C, and it has excellent heat resistance and chemical stability. The laminated paperboard products bonded by the adhesive of the present invention can meet the heat resistance requirements of Class F electrical insulation materials, and have high electrical strength, small shrinkage, good insulation, and overall performance better than the imported UHV transformer laminated paperboard products, solving a bottleneck problem in my country's power field.

[0017] 2. The present invention adopts a thermal curing process and can be produced using existing equipment.

[0018] 3. The resin adhesive in the adhesive component of the present invention does not contain accelerator components, and is difficult to react after being mixed with a curing agent at room temperature. It has an ultra-long operating time and can be completely cured in 1 to 2 hours after being heated to 100 to 120°C. It is very suitable for mass gluing, laminating, and curing laminated paperboards in production equipment, which is beneficial for manufacturers to improve production efficiency and reduce energy consumption. At the same time, no toxic or harmful substances will be released during the production of the adhesive. DETAILED DESCRIPTION

[0019] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific implementation methods. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not used to limit the present invention.

[0020] Example 1

[0021] Preparation method of phenolic epoxy vinyl ester resin: put 374 parts of NPPN-631 phenolic epoxy resin into a reactor, stir and heat to 80°C, then add 0.1 parts of stabilizer 2,5-di-tert-butylhydroquinone and 2 parts of N,N-dimethylaniline, and then drop 172 parts of methacrylic acid into the reactor within 2 hours. After the dropwise addition is completed, gradually increase the temperature to 110°C to obtain a reaction solution. When the acid value of the reaction solution drops to 13 mgKOH / g, cool to 80°C, add 274 parts of styrene, and obtain phenolic epoxy vinyl ester resin.

[0022] Preparation method of resin glue: 0.8 parts of polyamide wax, 0.2 parts of wetting and dispersing agent, 0.01 parts of defoaming agent, 30 parts of talcum powder and 7 parts of mica powder are added to 62 parts of phenolic epoxy vinyl ester resin in sequence, and the resin glue is obtained after stirring for 30 minutes.

[0023] The prepared resin glue and curing agent are mixed evenly in a weight ratio of 100:1, and allowed to stand for 20 minutes to defoam, thereby obtaining an adhesive. The curing agent is a methyl ethyl ketone peroxide solution with an active oxygen content of 9.1%.

[0024] Thermal curing process: Apply the above-mentioned adhesive on one side of a cardboard, and overlap another cardboard on the above-mentioned coated cardboard. After overlapping neatly, send it into the hot pressing equipment, gradually pressurize and heat it to a unit pressure of 3MPa and a temperature of 100℃, maintain it for 1h, and then gradually cool it down to 40℃. After releasing the pressure, the cardboard is bonded to obtain a UHV transformer laminated cardboard product.

[0025] Example 2

[0026] Preparation method of phenolic epoxy vinyl ester resin: put 396 parts of NPPN-638S phenolic epoxy resin into a reactor, stir and heat to 80°C, then add 0.1 parts of stabilizer tert-butylhydroquinone and 2 parts of N,N-dimethylaniline, and then drop 172 parts of methacrylic acid into the reactor within 2 hours. After the dropwise addition is completed, gradually increase the temperature to 110°C to obtain a reaction solution. When the acid value of the reaction solution drops to 15 mgKOH / g, cool to 80°C, add 284 parts of styrene, and obtain phenolic epoxy vinyl ester resin.

[0027] Preparation method of resin glue: 0.5 parts of organic bentonite, 0.1 parts of wetting and dispersing agent, 0.01 parts of defoaming agent, 30 parts of talc and 1.4 parts of kaolin are added in sequence to 68 parts of phenolic epoxy vinyl ester resin, and the resin glue is obtained after stirring for 40 minutes.

[0028] The prepared resin glue and curing agent are mixed evenly in a weight ratio of 100:2, and allowed to stand for 40 minutes to defoam, thereby obtaining an adhesive. The curing agent is a methyl ethyl ketone peroxide solution with an active oxygen content of 9.5%.

[0029] Thermal curing process: Apply the above-mentioned adhesive on one side of a cardboard, and overlap another cardboard on the above-mentioned coated cardboard. After overlapping neatly, send it into the hot pressing equipment, gradually pressurize and heat it to a unit pressure of 4MPa and a temperature of 110℃, maintain it for 1.5h, and then gradually cool it down to 40℃ to obtain the ultra-high voltage transformer laminated cardboard product.

[0030] Example 3

[0031] Preparation method of phenolic epoxy vinyl ester resin: put 440 parts of F-44 phenolic epoxy resin into a reactor, stir and heat to 80°C, then add 0.1 parts of stabilizer o-methyl hydroquinone and 2 parts of N, N-dimethylaniline, and then drop 172 parts of methacrylic acid into the reactor within 2 hours. After the dropwise addition is completed, gradually increase the temperature to 110°C to obtain a reaction solution. When the acid value of the reaction solution drops to 17 mgKOH / g, cool to 80°C, add 300 parts of styrene, and obtain phenolic epoxy vinyl ester resin.

[0032] Preparation method of resin glue: put 72 parts of phenolic epoxy vinyl ester resin into a reaction kettle, and then add 3 parts of organic bentonite, 0.1 parts of wetting dispersant, 20 parts of silica powder and 5 parts of kaolin in sequence, and stir for 60 minutes to obtain resin glue.

[0033] The prepared resin glue and curing agent are mixed evenly in a weight ratio of 100:3, and allowed to stand for 60 minutes to defoam, thereby obtaining an adhesive. The curing agent is a methyl ethyl ketone peroxide solution with an active oxygen content of 10%.

[0034] Thermal curing process: Apply the above-mentioned adhesive on one side of a cardboard, and overlap another cardboard on the above-mentioned coated cardboard. After overlapping neatly, send it into the hot pressing equipment, gradually pressurize and heat it to a unit pressure of 6MPa and a temperature of 120℃, maintain it for 2h, and then gradually cool it down to 40℃ to obtain the ultra-high voltage transformer laminated cardboard.

[0035] Comparative Example 1

[0036] The phenolic epoxy vinyl ester resin in Example 2 was replaced by epoxy vinyl ester resin, and the other steps were the same as Example 2.

[0037] Comparative Example 2

[0038] Put 68 parts of unsaturated polyester resin into a reactor, add 0.5 parts of organic bentonite, 0.1 parts of wetting and dispersing agent, 0.01 parts of defoaming agent, 30 parts of talcum powder and 1.4 parts of kaolin in turn, stir for 40 minutes to obtain resin glue; mix the above-prepared resin glue and curing agent in a weight ratio of 100:2, the curing agent is a methyl ethyl ketone peroxide solution with an active oxygen content of 9.5%, stand for 40 minutes to defoam, and obtain adhesive. Then apply the above adhesive on one side of a cardboard, and overlap another cardboard on the above-coated cardboard, and send it to the hot pressing equipment after overlapping neatly, gradually pressurize to a unit pressure of 4MPa, maintain for 6 hours, release the pressure and place it for 24 hours to obtain laminated cardboard.

[0039] The resin adhesive and laminated paperboard products prepared in the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1 below.

[0040] As can be seen from Table 1, the bending strength, shrinkage rate and room temperature inner layer strength of the samples of Example 1, Example 2 and Example 3 are better than those of the samples of Comparative Example 1 and Comparative Example 2, and the operable time is much longer than that of the samples of Comparative Example 1 and Comparative Example 2. The electrical strength and conductivity are also better than those of the samples of Comparative Example 1 and Comparative Example 2. Moreover, compared with Comparative Example 1 and Comparative Example 2, the performance of Example 1, Example 2 and Example 3 is extremely excellent in terms of the thermal deformation temperature of the resin glue sample and the inner layer strength retention rate of the prepared laminated paperboard sample under high temperature conditions of 160°C.

[0041] In addition, in a longitudinal comparison, the performance of the samples of Example 1, Example 2, and Example 3 after oil immersion is basically not reduced compared with the standard conditions, the shear strength under the high temperature condition of 120°C is more than 90% of the shear strength under the normal temperature condition, and the shear strength under the high temperature condition of 160°C is more than 80% of the shear strength under the normal temperature condition, indicating that the laminated paperboards prepared in Example 1, Example 2, and Example 3 have excellent high temperature resistance and stable performance in transformer oil, and can meet the use requirements of UHV transformers.

[0042] On the whole, the adhesive prepared with phenolic epoxy vinyl ester resin as the main component and the curing process used for cardboard bonding in the present invention have a significant effect on improving the performance of laminated cardboard products for ultra-high voltage transformers.

[0043] Table 1 Test data results of examples and comparative examples

[0044]

[0045] It can be understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. An adhesive for ultra-high voltage transformer laminated paperboard, characterized in that: The adhesive is composed of a resin glue and a curing agent, and the weight ratio of the resin glue to the curing agent is 100:1-3; the resin glue has the following components in parts by weight:

2. The adhesive for ultra-high voltage transformer laminated paperboard according to claim 1, characterized in that: The phenolic epoxy vinyl ester resin is prepared according to the following steps: according to parts by weight, 374 to 440 parts of phenolic epoxy resin are put into a reaction kettle, stirred and heated to 80°C, then 0.1 parts of a stabilizer and 2 parts of N,N-dimethylaniline are added, and then 172 parts of methacrylic acid are dripped into the reaction kettle within 2 hours. After the dripping is completed, the temperature is raised to 110°C to obtain a reaction solution. When the acid value of the reaction solution is 13 to 17 mgKOH / g, the temperature is lowered to 80°C, and 274 to 300 parts of styrene are added to obtain the phenolic epoxy vinyl ester resin.

3. The adhesive for ultra-high voltage transformer laminated paperboard according to claim 2, characterized in that: The brand of the phenolic epoxy resin is at least one of NPPN-631, NPPN-638S, F-44 and F-51.

4. The adhesive for ultra-high voltage transformer laminated paperboard according to claim 2, characterized in that: The stabilizer is at least one of o-methyl hydroquinone, tert-butyl hydroquinone and 2,5-di-tert-butyl hydroquinone.

5. The adhesive for ultra-high voltage transformer laminated paperboard according to claim 1, characterized in that: The anti-settling agent is at least one of organic bentonite, fumed silica and polyamide wax.

6. The adhesive for ultra-high voltage transformer laminated paperboard according to claim 1, characterized in that: The insulating filler is at least one of talc powder, silica powder, mica powder and kaolin.

7. The adhesive for ultra-high voltage transformer laminated paperboard according to claim 1, characterized in that: The curing agent is a methyl ethyl ketone peroxide solution, and the active oxygen content of the methyl ethyl ketone peroxide solution is 9.1-10%.

8. A method for preparing an adhesive for ultra-high voltage transformer laminated paperboard, characterized in that: The preparation method is as follows: phenolic epoxy vinyl ester resin is placed in a reaction kettle, an anti-settling agent, a wetting dispersant, a defoaming agent and an insulating filler are added in sequence, and a resin glue is obtained after stirring for 30 to 60 minutes, and the resin glue and a curing agent are mixed evenly, and the mixture is allowed to stand for 20 to 60 minutes to defoam, so as to obtain an adhesive, wherein the components of the resin glue and the ratio of the resin glue to the curing agent are the same as the ratio of the components in claim 1.

9. Use of the adhesive according to any one of claims 1 to 7 in bonding laminated paperboards for ultra-high voltage transformers, characterized in that: The adhesive described in claim 1 is evenly applied on the cardboard by single-sided coating, and then another cardboard is overlapped on the cardboard coated with the adhesive, and the number of times the above operation is repeated is determined according to the number of layers of cardboard to be prepared, and then the neatly overlapped cardboard is sent to a hot pressing device, and maintained for 1 to 2 hours under the conditions of a unit pressure of 3 to 6 MPa and a temperature of 100 to 120° C., and then cooled to 40° C. and released to normal pressure, so that the bonding of the cardboard is completed, and a laminated cardboard for a UHV transformer is obtained.