Flame-retardant silane modified polyether sealant and preparation method thereof
By using N,P doped carbon quantum dots as flame retardant in silane modified polyether sealant, the problem of flammability of silane modified polyether sealant is solved, and both flame retardant and mechanical properties are achieved. Suitable for bonding and sealing of a variety of substrates.
Patent Information
- Application Number
- CN202411424367.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
AI Technical Summary
Silane modified polyether sealants lack flame retardant properties and are flammable, which limits their wide application.
Using N,P doped carbon quantum dots as flame retardant, combined with silane-modified polyether polymer, calcium carbonate, plasticizer, etc., the flame retardant type silane-modified polyether sealant is prepared by vacuum stirring and heating. , balance its flame retardant effect and mechanical properties.
Prepare a silane modified polyether sealant with excellent flame retardant properties and good mechanical properties, which can maintain strong tensile strength and elongation of break under good flame retardant effects, and is suitable for the adhesion of a variety of substrates. Connect and seal.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical materials, and in particular to a flame retardant silane-modified polyether sealant and a preparation method thereof. Background Art
[0002] Silane modified polyether sealant (MS sealant) is a single-component or two-component elastic sealant based on MS polymer as the base polymer, combined with fillers, plasticizers and other functional additives. MS polymer is a cross-linked polymer based on silane-terminated polyether. MS polymer-based products do not contain silicone components and solvents, nor do they contain polyurethane groups. Most formulations are odorless and environmentally friendly. The inherent elasticity of MS adhesives and sealants can absorb and compensate for dynamic loads, evenly transfer forces, and prevent premature fatigue of materials. MS sealant materials can achieve bonding between a variety of substrates and have excellent adhesion, coating, durability, resistance to deformation and displacement, and environmental friendliness. With the further development of MS sealant research and development and the continuous development of the market, the application of MS sealants has expanded from waterproofing and sealing in the traditional construction field to sealing and bonding in more fields such as home improvement, transportation, electronics and electrical appliances.
[0003] However, MS sealants are not flame retardant and are flammable when exposed to open flames, which obviously limits their widespread application. Therefore, it is very necessary to develop a MS sealant with flame retardant function. At present, there are some MS sealants that use intumescent flame retardants as flame retardants, but the flame retardant properties and mechanical properties are still lacking. Carbon nanomaterials are widely used in the flame retardant modification of polymers due to their abundant sources, diverse preparation methods, and excellent flame retardant properties. Carbon dots (CDs), as zero-dimensional carbon nanomaterials, are widely available, simple to prepare, very easy to be compatible with composite materials, and green and environmentally friendly. Therefore, using carbon dots as flame retardants to develop a MS sealant with flame retardant properties can solve the above technical problems. Summary of the invention
[0004] The main purpose of the present invention is to provide a flame retardant silane modified polyether sealant, using N, P doped carbon quantum dots (N, P@CDs) as flame retardants, the prepared flame retardant MS sealant has good mechanical properties and excellent flame retardant properties.
[0005] To achieve the above object, the present invention provides a flame retardant silane-modified polyether sealant, comprising the following components in parts by weight:
[0006]
[0007] The flame retardant is N, P doped carbon quantum dots. Preferably, the N, P doped carbon quantum dots are prepared from a carbon source, a phosphorus source and a solvent as raw materials.
[0008] The present invention uses N, P doped carbon quantum dots as flame retardants and MS polymer as base glue to prepare flame retardant silane modified polyether sealant, which can obtain green and environmentally friendly MS sealant with good flame retardancy. By adjusting the amount of N, P@CDs, the mechanical properties and flame retardant effect of the sealant are balanced, so that it has a good flame retardant effect, strong tensile strength and elongation at break, and maintains good mechanical properties.
[0009] Conventional plasticizers, coupling agents, catalysts, and thixotropic agents can all be used in the present invention.
[0010] Preferably, the plasticizer includes but is not limited to at least one of polypropylene glycol 3000, polypropylene glycol 2000 and polypropylene glycol 1000.
[0011] The coupling agent includes but is not limited to at least one of KH792, KH540, KH550 and KH560.
[0012] The catalyst includes, but is not limited to, at least one of dibutyltin dilaurate and dibutyltin diacetate.
[0013] The thixotropic agent includes, but is not limited to, at least one of fumed silica and hydrogenated castor oil.
[0014] Preferably, the carbon source comprises one or more of lignin, sodium lignin sulfonate, alkali lignin, urea, piperazine, melamine, and imidazole-based ionic liquid.
[0015] Preferably, the phosphorus source includes one or more of phosphoric acid, piperazine pyrophosphate, ammonium polyphosphate, polyphosphazene, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-sulfide.
[0016] Preferably, the solvent includes any one of ethanol, methanol, water and sulfuric acid.
[0017] Preferably, the carbon source is 1.0-10.0 g; the phosphorus source is 1.0-10.0 g; and the solvent is 10.0-50.0 mL.
[0018] Preferably, the carbon source is 8.0-10.0 g; the phosphorus source is 2.0-5.0 g; the solvent is 50.0 mL; the carbon source is a mixture of urea, melamine and imidazole ionic liquid, the phosphorus source is a mixture of phosphoric acid and ammonium polyphosphate, and the solvent is methanol. The flame-retardant silane-modified polyether sealant prepared by this raw material ratio has good flame retardant properties and good mechanical properties.
[0019] The present invention also provides a method for preparing the flame-retardant silane-modified polyether sealant, comprising the following steps:
[0020] S1. Preparation of N and P doped carbon quantum dots;
[0021] S2, mixing the silane-modified polyether polymer, calcium carbonate, plasticizer and the N, P-doped carbon quantum dots according to the formula amount at 100-120° C., removing water and cooling to room temperature to obtain a mixed slurry;
[0022] S3, adding a coupling agent, a catalyst, and a thixotropic agent to the mixed slurry, and stirring in vacuum until the reaction is completed, thereby obtaining the flame-retardant silane-modified polyether sealant;
[0023] The preparation of the N and P doped carbon quantum dots comprises the following steps:
[0024] 1) dissolving a carbon source and a phosphorus source in a solvent according to a ratio to obtain a mixed solution;
[0025] 2) placing the mixed solution in a reaction kettle and heating it;
[0026] 3) After the reaction is completed, the solution is taken out after cooling and freeze-dried to obtain the N, P doped carbon quantum dots. Preferably, in the above preparation method, the heating temperature in step S1 is 160-200°C and the heating time is 5-12h; the vacuum degree in step S2 and step S3 is not less than -0.09MPa.
[0027] Compared with the prior art, the beneficial effects of the present invention include at least: by adding N, P-doped carbon quantum dots as flame retardants in silane-modified polyether sealants, the present invention has a simple preparation process, is green and environmentally friendly, and can prepare flame-retardant silane-modified polyether sealants with excellent flame retardant properties and good mechanical properties. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0029] A method for preparing a flame retardant silane-modified polyether sealant comprises the following steps:
[0030] S1. Preparation of N, P-doped carbon quantum dots:
[0031] 1) Dissolve the carbon source and the phosphorus source in a solvent according to a ratio to obtain a mixed solution; wherein the carbon source is 1.0-10.0 g; the phosphorus source is 1.0-10.0 g; and the solvent is 10-50.0 mL. Preferably, the carbon source is 8.0-10.0 g; the phosphorus source is 2.0-5.0 g; and the solvent is 50.0 mL.
[0032] 2) placing the mixed solution in a reaction kettle and heating it at a temperature of 160 to 200° C. for 5 to 12 hours.
[0033] 3) After the reaction is completed, the solution is taken out after cooling and freeze-dried to obtain the N, P-doped carbon quantum dots;
[0034] S2, silane-modified polyether polymer, calcium carbonate, plasticizer, N, P-doped carbon quantum dots are stirred at 100-120°C, speed 500r / min, vacuum (vacuum degree not less than -0.09MPa) for 1h according to the formula, and then water is removed. After the reaction is completed, the mixture is cooled to room temperature to obtain a mixed mortar;
[0035] S3. After adding coupling agent, catalyst and thixotropic agent to the mixed slurry, evacuate to -0.09MPa, rotate at 300-400r / min, stir in vacuum for 10min, adjust the rotation speed to 500r / min, stir for 20min, until the reaction is completed, and obtain the flame-retardant silane-modified polyether sealant.
[0036] The flame retardant silane modified polyether sealant comprises the following components in parts by weight:
[0037]
[0038] Conventional plasticizers, coupling agents, catalysts, and thixotropic agents can all be used in the present invention.
[0039] Preferably, the plasticizer includes but is not limited to at least one of polypropylene glycol 3000, polypropylene glycol 2000 and polypropylene glycol 1000.
[0040] The coupling agent includes but is not limited to at least one of KH792, KH540, KH550 and KH560.
[0041] The catalyst includes, but is not limited to, at least one of dibutyltin dilaurate and dibutyltin diacetate.
[0042] The thixotropic agent includes but is not limited to at least one of fumed silica and hydrogenated castor oil. Preferably, the carbon source includes one or more of lignin, sodium lignin sulfonate, alkali lignin, urea, piperazine, melamine, and imidazole-based ionic liquids. Preferably, the carbon source includes a mixture of urea, melamine, and imidazole-based ionic liquids.
[0043] Preferably, the phosphorus source comprises one or more of phosphoric acid, piperazine pyrophosphate, ammonium polyphosphate, polyphosphazene, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-sulfide. Preferably, the phosphorus source comprises a mixture of phosphoric acid and ammonium polyphosphate.
[0044] Preferably, the solvent includes any one of ethanol, methanol, water and sulfuric acid. Preferably, the solvent is methanol.
[0045] The present invention is further described below by enumerating examples. It should be understood that the following examples are only used to illustrate the present invention, but not to limit the present invention. In the absence of special instructions, the parts are all parts by weight.
[0046] Example 1
[0047] A series of flame retardant silane modified polyether sealants are provided, which are prepared by using the raw material formulas in Tables 1 and 2 according to a method comprising the following steps:
[0048] S1. Preparation of N, P-doped carbon quantum dots:
[0049] 1) dissolving a carbon source and a phosphorus source in a solvent according to a ratio to obtain a mixed solution;
[0050] 2) placing the mixed solution in a reaction kettle and heating it at 180° C. for 8 h.
[0051] 3) After the reaction is completed, the solution is taken out after cooling and freeze-dried to obtain the N, P-doped carbon quantum dots;
[0052] S2, silane-modified polyether polymer, calcium carbonate, plasticizer, N, P-doped carbon quantum dots are stirred at 100°C, 500r / min, vacuum (vacuum degree not less than -0.09MPa) for 1h according to the formula, and then water is removed. After the reaction is completed, the mixture is cooled to room temperature to obtain a mixed slurry;
[0053] S3. After adding coupling agent, catalyst and thixotropic agent to the mixed slurry, evacuate to -0.09MPa, rotate at 350r / min, stir in vacuum for 10min, adjust the rotation speed to 500r / min, stir for 20min, until the reaction is completed, and obtain the flame-retardant silane-modified polyether sealant.
[0054] Example 2
[0055] A series of flame retardant silane modified polyether sealants are provided, which are prepared by using the raw material formulas in Tables 1 and 2 according to a method comprising the following steps:
[0056] S1. Preparation of N, P-doped carbon quantum dots:
[0057] 1) dissolving a carbon source and a phosphorus source in a solvent according to a ratio to obtain a mixed solution;
[0058] 2) placing the mixed solution in a reaction kettle and heating it at 180° C. for 8 h.
[0059] 3) After the reaction is completed, the solution is taken out after cooling and freeze-dried to obtain the N, P-doped carbon quantum dots;
[0060] S2, silane-modified polyether polymer, calcium carbonate, plasticizer, N, P-doped carbon quantum dots are stirred at 100°C, 500r / min, vacuum (vacuum degree not less than -0.09MPa) for 1h according to the formula, and then water is removed. After the reaction is completed, the mixture is cooled to room temperature to obtain a mixed slurry;
[0061] S3. After adding coupling agent, catalyst and thixotropic agent to the mixed slurry, evacuate to -0.09MPa, rotate at 350r / min, stir in vacuum for 10min, adjust the rotation speed to 500r / min, stir for 20min, until the reaction is completed, and obtain the flame-retardant silane-modified polyether sealant.
[0062] Example 3
[0063] A series of flame retardant silane modified polyether sealants are provided, which are prepared by using the raw material formulas in Tables 1 and 2 according to a method comprising the following steps:
[0064] S1. Preparation of N, P-doped carbon quantum dots:
[0065] 1) dissolving a carbon source and a phosphorus source in a solvent according to a ratio to obtain a mixed solution;
[0066] 2) placing the mixed solution in a reaction kettle and heating it at 180° C. for 8 h.
[0067] 3) After the reaction is completed, the solution is taken out after cooling and freeze-dried to obtain the N, P-doped carbon quantum dots;
[0068] S2, silane-modified polyether polymer, calcium carbonate, plasticizer, N, P-doped carbon quantum dots are stirred at 100°C, 500r / min, vacuum (vacuum degree not less than -0.09MPa) for 1h according to the formula, and then water is removed. After the reaction is completed, the mixture is cooled to room temperature to obtain a mixed slurry;
[0069] S3. After adding coupling agent, catalyst and thixotropic agent to the mixed slurry, evacuate to -0.09MPa, rotate at 350r / min, stir in vacuum for 10min, adjust the rotation speed to 500r / min, stir for 20min, until the reaction is completed, and obtain the flame-retardant silane-modified polyether sealant.
[0070] Example 4
[0071] A series of flame retardant silane modified polyether sealants are provided, which are prepared by using the raw material formulas in Tables 1 and 2 according to a method comprising the following steps:
[0072] S1. Preparation of N, P-doped carbon quantum dots:
[0073] 1) dissolving a carbon source and a phosphorus source in a solvent according to a ratio to obtain a mixed solution;
[0074] 2) placing the mixed solution in a reaction kettle and heating it at 180° C. for 8 h.
[0075] 3) After the reaction is completed, the solution is taken out after cooling and freeze-dried to obtain the N, P-doped carbon quantum dots;
[0076] S2, silane-modified polyether polymer, calcium carbonate, plasticizer, N, P-doped carbon quantum dots are stirred at 100°C, 500r / min, vacuum (vacuum degree not less than -0.09MPa) for 1h according to the formula, and then water is removed. After the reaction is completed, the mixture is cooled to room temperature to obtain a mixed slurry;
[0077] S3. After adding coupling agent, catalyst and thixotropic agent to the mixed slurry, evacuate to -0.09MPa, rotate at 350r / min, stir in vacuum for 10min, adjust the rotation speed to 500r / min, stir for 20min, until the reaction is completed, and obtain the flame-retardant silane-modified polyether sealant.
[0078] Example 5
[0079] A series of flame retardant silane modified polyether sealants are provided, which are prepared by using the raw material formulas in Tables 1 and 2 according to a method comprising the following steps:
[0080] S1. Preparation of N, P-doped carbon quantum dots:
[0081] 1) dissolving a carbon source and a phosphorus source in a solvent according to a ratio to obtain a mixed solution;
[0082] 2) placing the mixed solution in a reaction kettle and heating it at 180° C. for 8 h.
[0083] 3) After the reaction is completed, the solution is taken out after cooling and freeze-dried to obtain the N, P-doped carbon quantum dots;
[0084] S2, silane-modified polyether polymer, calcium carbonate, plasticizer, N, P-doped carbon quantum dots are stirred at 180°C, 500r / min, vacuum (vacuum degree not less than -0.09MPa) for 1h according to the formula, and then water is removed. After the reaction is completed, the mixture is cooled to room temperature to obtain a mixed mortar;
[0085] S3. After adding coupling agent, catalyst and thixotropic agent to the mixed slurry, evacuate to -0.09MPa, rotate at 350r / min, stir in vacuum for 10min, adjust the rotation speed to 500r / min, stir for 20min, until the reaction is completed, and obtain the flame-retardant silane-modified polyether sealant.
[0086] Table 1 Raw material composition of N, P doped carbon quantum dots in Examples 1 to 5
[0087]
[0088] Table 2 Raw material composition of flame retardant silane modified polyether sealant of Examples 1 to 5 (parts by weight)
[0089]
[0090]
[0091] Blank example
[0092] The same raw material formula as in Example 3 was used, except that N,P@CDs was not added.
[0093] The preparation process is as follows:
[0094] A silane-modified polyether sealant is prepared according to a method comprising the following steps:
[0095] S1. Stir silane-modified polyether polymer, calcium carbonate and plasticizer according to the formula at 100°C, 500r / min, vacuum (vacuum degree not less than -0.09MPa) for 1h, and remove water. After the reaction is completed, cool to room temperature to obtain a mixed mortar;
[0096] S2. After adding coupling agent, catalyst and thixotropic agent to the mixed slurry, evacuate to -0.09 MPa, rotate at 350 r / min, stir in vacuum for 10 min, adjust the rotation speed to 500 r / min, stir for 20 min, until the reaction is completed, and obtain the silane-modified polyether sealant.
[0097] Performance Testing
[0098] The performance tests of all embodiments of the present invention adopt the following test items and methods:
[0099] 1. Flame retardant performance: The flame retardant performance of the sealant is tested according to the requirements of the standard "GB / T 24267-2009".
[0100] 2. Mechanical properties: The tensile strength and elongation at break of the sealant are tested according to the standard "GB / T 528-2009".
[0101] The properties of the flame retardant silane modified polyether sealants prepared in Examples 1 to 5 and the blank example were tested. The test results are shown in Table 3.
[0102] Table 3 Test results of Examples 1 to 5 and blank examples
[0103]
[0104]
[0105] It can be seen from Table 3 that the flame retardancy of Examples 1 to 5 reaches V0, and the flame retardancy of the blank example is poor. It should be noted that Examples 1 to 5 only exemplarily show plasticizers, coupling agents, catalysts and thixotropic agents, and when other preferred plasticizers, coupling agents, catalysts and thixotropic agents described in the present invention are used, the same technical effects are achieved.
[0106] Example 6
[0107] The same raw material composition and process parameters as in Example 1 were used, except that the amount of N,P@CDs was adjusted as shown in the following table (parts by weight):
[0108] Example 6-1 Example 6-2 Example 6-3 Example 6-4 N,P@CDs 5 7.5 12.5 15
[0109] Comparative Example 1
[0110] The same raw material composition and process parameters as in Example 1 were used, except that the amount of N,P@CDs was adjusted as shown in the following table (parts by weight):
[0111] Comparative Example 1 N,P@CDs 20
[0112] The properties of the flame retardant silane-modified polyether sealants prepared in Example 6 and Comparative Example 1 were tested, and the test results are shown in Table 4.
[0113] Table 4 Test results of Example 1, Example 6 and Comparative Example 1
[0114]
[0115] As shown in Table 4, with the increase of N,P@CDs dosage, the tensile strength of the sealant gradually increases, and the elongation at break gradually decreases; when the dosage of flame retardant N,P@CDs is 15 parts, the extrusion of the sealant begins to deteriorate. It can be seen that with the increase of N,P@CDs, the flame retardant grade increases, but the mechanical properties decrease. Therefore, adjusting the appropriate amount of N,P@CDs can better balance the flame retardant and mechanical properties. It can be inferred that due to the small particle size and high activity of flame retardant N,P@CDs, it can be evenly dispersed in the sealant system and have a strong interaction with the sealant. According to Examples 6-1 and 6-2, it can be seen that when the amount of flame retardant is 5 to 7.5 parts, the flame retardant properties can only reach V2 and V1 levels. This shows that when the amount of flame retardant added is 10 to 15 parts, the flame retardant properties reach the best V0 level, and when the amount of flame retardant added is 10 to 12.5 parts, it can ensure good extrusion and mechanical properties. Among them, especially when the amount of flame retardant is 10 parts, the comprehensive performance of the sealant is optimal, achieving the best flame retardant properties while having suitable tensile strength and elongation at break.
[0116] Example 7
[0117] The same raw material composition and process parameters as in Example 1 are used, except that the raw material formula of N,P@CDs is adjusted as shown in the following table):
[0118]
[0119] Comparative Example 2
[0120] The same raw material composition and process parameters as in Example 1 are used, except that the raw material formula of N,P@CDs is adjusted as shown in the following table:
[0121]
[0122] The properties of the flame retardant silane modified polyether sealants prepared in Example 7 and Comparative Example 2 were tested. The test results are shown in Tables 5 and 6.
[0123] Table 5 Test results of Example 1 and Example 7
[0124]
[0125] Table 6 Test results of comparative example 2
[0126] Comparative Example 2-1 Comparative Example 2-2 Comparative Examples 2-3 Tensile strength / MPa 0.88 0.94 0.79 Elongation at break / % 610 573 659 Extrusion excellent excellent excellent Oxygen Index 23 28 24 Flame retardant grade <![CDATA[V2]]> <![CDATA[V1]]> <![CDATA[V2]]>
[0127] From the results of Table 3, Table 5 and Table 6, it can be seen that the flame retardant properties and mechanical properties of silane-modified polyether sealant can be adjusted by changing the composition of carbon dot raw materials, so that the two are balanced with each other and the comprehensive performance is the best. From Table 3, it can be seen that when the carbon source is a mixture of urea, melamine and imidazole-based ionic liquid, the phosphorus source is a mixture of phosphoric acid and ammonium polyphosphate, and the solvent is methanol, the silane-modified polyether sealant has the best comprehensive performance. From the comparison of the results of Table 5 and Table 6, it can be seen that when the carbon source is 8.0-10.0g, the phosphorus source is 2.0-5.0g, and the solvent is 50mL, the flame retardant grade is the best, which can reach V0, and the mechanical properties are good and stable. Among them, when the weight ratio of urea: melamine: imidazole-based ionic liquid is 2-8: 1-4: 1-3, and the weight ratio of phosphoric acid: ammonium polyphosphate is 1-3: 1-4, the above raw material ratio can obtain the best flame retardant and mechanical properties.
[0128] In summary, the present invention adds N, P@CDs to the silane-modified polyether sealant to make it flame retardant. After the amount of N, P@CDs is preferably limited, it can have good flame retardant properties and good mechanical properties. From the results of Example 7, it can be seen that after the raw material formula of N, P@CDs is preferably limited, the flame retardant effect of MS sealant can be further improved.
[0129] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A flame retardant silane-modified polyether sealant, characterized in that: The composition comprises the following components in parts by weight: The flame retardant is N, P doped carbon quantum dots.
2. A flame retardant silane-modified polyether sealant as claimed in claim 1, characterized in that: The N, P doped carbon quantum dots are prepared from a carbon source, a phosphorus source and a solvent as raw materials.
3. The flame retardant silane-modified polyether sealant according to claim 1, characterized in that: The plasticizer includes at least one of polypropylene glycol 3000, polypropylene glycol 2000 and polypropylene glycol 1000; the coupling agent includes at least one of KH792, KH540, KH550 and KH560; the catalyst includes at least one of dibutyltin dilaurate and dibutyltin diacetate; the thixotropic agent includes at least one of fumed silica and hydrogenated castor oil.
4. The flame retardant silane-modified polyether sealant according to claim 2, characterized in that: The carbon source includes one or more of lignin, sodium lignin sulfonate, alkali lignin, urea, piperazine, melamine, and imidazole-based ionic liquid.
5. The flame retardant silane-modified polyether sealant according to claim 2, characterized in that: The phosphorus source includes one or more of phosphoric acid, piperazine pyrophosphate, ammonium polyphosphate, polyphosphazene, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-sulfide.
6. The flame retardant silane-modified polyether sealant according to claim 2, characterized in that: The solvent includes any one of ethanol, methanol, water and sulfuric acid.
7. The flame retardant silane-modified polyether sealant according to claim 2, characterized in that: The carbon source is 0.1-10.0 g; the phosphorus source is 0.1-10.0 g; and the solvent is 10.0-50.0 mL.
8. The flame retardant silane-modified polyether sealant according to claim 2, characterized in that: The carbon source is 8.0-10.0 g; the phosphorus source is 2.0-5.0 g; the solvent is 50.0 mL; The carbon source is a mixture of urea, melamine and imidazole-based ionic liquid, the phosphorus source is a mixture of phosphoric acid and ammonium polyphosphate, and the solvent is methanol.
9. The method for preparing the flame-retardant silane-modified polyether sealant according to any one of claims 2 to 8, characterized in that: The steps include: S1. Preparation of N and P doped carbon quantum dots; S2, mixing the silane-modified polyether polymer, calcium carbonate, plasticizer and the N, P-doped carbon quantum dots according to the formula amount at 100-120° C., removing water and cooling to room temperature to obtain a mixed slurry; S3, adding a coupling agent, a catalyst, and a thixotropic agent to the mixed slurry, and stirring in vacuum until the reaction is completed, thereby obtaining the flame-retardant silane-modified polyether sealant; Wherein, the preparation of the N, P doped carbon quantum dots comprises the following steps: 1) dissolving a carbon source and a phosphorus source in a solvent according to a ratio to obtain a mixed solution; 2) placing the mixed solution in a reaction kettle and heating it; 3) After the reaction is completed, the solution is taken out after cooling and freeze-dried to obtain the N, P-doped carbon quantum dots.
10. The method for preparing the flame-retardant silane-modified polyether sealant according to claim 9, characterized in that: The heating temperature in step S1 is 160-200° C. and the heating time is 5-12 hours; The vacuum degree in step S2 and step S3 is not less than -0.09 MPa.
Citation Information