Cr < 3 + >-doped phosphate near-infrared fluorescent powder as well as preparation method and application thereof
Through the preparation of Cr3+ doped phosphate near-infrared phosphor, the problem of near-infrared light emission in the range of 750nm-900nm under blue light excitation is solved, and an efficient near-infrared light source material is realized, with wide application value and feasibility of industrial production.
Patent Information
- Application Number
- CN202411128089.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art lacks phosphate near-infrared phosphor materials that can efficiently emit near-infrared light in the range of 750nm-900nm under blue light excitation, which limits the development and application of near-infrared light sources.
The chemical formula of Cr3+ doped phosphate near-infrared phosphor is CdTi4(PO4)6:xCr3+, prepared by sintering and grinding, the main emission peak is in the range of 750nm-900nm and can be excited by blue light, and the value range of x is preferably 0.05≤x≤0.13 to improve luminous performance.
The prepared Cr3+ doped phosphate near-infrared phosphor has important application value in food detection, face recognition, safety monitoring, unmanned driving and other fields. The raw materials are cheap, the preparation process is simple, the product quality is stable, and it is suitable for industrial production.
Smart Images

Figure CN119081692A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to a Cr 3+ Phosphate-doped near-infrared phosphor and its preparation method and application. Background Art
[0002] Near-infrared (NIR) light sources have the characteristics of strong penetration, fast response speed, and non-destructive detection. They have important application value in many fields such as food inspection, face recognition, security monitoring, unmanned driving, agriculture, etc. However, in order to make them widely used, it is urgent to develop miniaturized, fast-responding, high-efficiency, broadband near-infrared light sources. Compared with traditional near-infrared luminescent materials, fluorescence-converted near-infrared light-emitting diodes (NIR pc-LEDs) have attracted much attention due to their small size, long life, low cost, high luminous efficiency, and adjustable spectrum. At present, although various new near-infrared luminescent materials have been developed, there is still a lack of materials with high blue light absorption and wide-band luminescence.
[0003] The Chinese patent application document with publication number CN116120928A discloses an ultra-wideband emission near-infrared phosphor and its preparation method, which belongs to the technical field of ultra-wideband near-infrared luminescent materials. The ultra-wideband emission near-infrared phosphor is based on K2SrGe8O 18 As the matrix material, Cr 3+ To activate the ions, Li + Ion, Li + With Cr 3+ Co-substitution of Ge in the matrix material 4+ , forming a solid solution. The preparation method includes the following steps: S1, weighing the raw materials according to the stoichiometric ratio of the elements, adding anhydrous ethanol, and grinding and mixing them evenly; S2, transferring the fully mixed raw materials to an alumina crucible for sintering to obtain a sintered sample; S3, after cooling the sintered sample to room temperature, taking out the sintered sample and grinding it to obtain an ultra-wideband emission near-infrared phosphor. The emission range covers 650-1200nm, and the half-peak width FWHM is 222nm. However, the patent does not disclose the Cr 3+ Doped phosphate near-infrared phosphors. Summary of the invention
[0004] The technical problem to be solved by the present invention is how to provide a blue light excited phosphate near-infrared phosphor and a preparation method thereof.
[0005] The present invention solves the above technical problems through the following technical means:
[0006] The first aspect of the present invention provides a Cr 3+Doped phosphate near-infrared phosphor, the chemical general formula of the near-infrared phosphor is CdTi4(PO4)6:xCr 3+ ; where x represents the molar fraction, and the value range of x is: 0 < x ≤ 0.2; the emission peak of the near-infrared phosphor is between 750 nm and 900 nm and can be excited by blue light.
[0007] Preferably, the value range of x is: 0.05 ≤ x ≤ 0.13. Within this range, the obtained near-infrared phosphor has more excellent luminescence performance.
[0008] Preferably, the wavelength of the blue light is 450 nm to 480 nm.
[0009] In the second aspect of the present invention, a preparation method of the above-mentioned Cr 3+ doped phosphate near-infrared phosphor is proposed, including the following steps:
[0010] (1) Sinter a mixture containing a Cd source, a Ti source, a Cr source, and a P source to obtain a sintered body;
[0011] The Cd source is selected from at least one of Cd oxides and nitrates; the Cr source is selected from at least one of Cr oxides and Cr nitrates; the Ti source is selected from at least one of Ti oxides and Ti nitrates; the P source is selected from at least one of P oxides and P phosphates;
[0012] (2) Grind the sintered body sufficiently to obtain the near-infrared phosphor.
[0013] Preferably, the sintering in step (1) is specifically: first perform sintering I, cool to obtain a pre-sintered body, and then perform sintering II to obtain a sintered body.
[0014] Preferably, the conditions for sintering I are: the temperature is 600 °C to 800 °C, and the time is 3 to 8 h; more preferably 700 °C, 5 h.
[0015] Preferably, before sintering I, the mixture is ground sufficiently; the particle size of the ground mixture is preferably 200 mesh to 600 mesh.
[0016] Preferably, the conditions for sintering II are: the temperature is 1200 °C to 1400 °C, and the time is 3 to 8 h; more preferably 1300 °C, and the time is 5 h.
[0017] Preferably, before sintering II, the pre-sintered body is ground sufficiently.
[0018] Preferably, the grinding time is 15 to 30 minutes each time.
[0019] Preferably, the heating rates of sintering I and sintering II are independently selected from 3 to 5° C. / min.
[0020] Preferably, the sintering I and sintering II are carried out in an air atmosphere.
[0021] Preferably, in step (2), the sintered body is ground to a particle size of 80-400 mesh.
[0022] The third aspect of the present invention proposes any one of the above Cr 3+ Application of phosphate-doped near-infrared phosphor or phosphate near-infrared phosphor prepared by any of the above methods in preparing near-infrared LED light sources.
[0023] The advantages of the present invention are:
[0024] 1) The phosphate near-infrared phosphor prepared by the present invention has important application value in many fields such as food detection, face recognition, security monitoring, unmanned driving, agriculture, etc.
[0025] 2) The raw materials used in the present invention are cheap, and the preparation process only requires a solid phase reaction at a relatively low temperature. The process is simple, and the quality of the obtained product is stable and reliable, which is very conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is an X-ray diffraction pattern of the phosphate near-infrared phosphor prepared in Example 2 of the present invention;
[0027] Figure 2 This is an excitation spectrum diagram of the phosphate near-infrared phosphor prepared in Example 2 of the present invention;
[0028] Figure 3 This is an emission spectrum of the phosphate near-infrared phosphor prepared in Example 2 of the present invention;
[0029] Figure 4 This is a temperature-dependent spectral intensity trend diagram of the phosphate near-infrared phosphor prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0030] The present application is described in detail below in conjunction with implementation cases, but the present application is not limited to these implementation cases.
[0031] The present application discloses a method for preparing a phosphate near-infrared phosphor, comprising the following steps:
[0032] 1) weighing raw materials in a certain stoichiometric ratio and grinding and mixing them thoroughly to obtain a mixture;
[0033] 2) sintering the mixture once or multiple times in an air atmosphere to obtain a sintered body;
[0034] 3) Grind the sintered body thoroughly to obtain phosphate near-infrared phosphor.
[0035] Wherein, in step 1), the reaction raw materials are weighed according to the stoichiometric ratio of CdTi4(PO4)6. Commercially available micron-grade or nano-grade raw materials with a purity of more than 99% can be used without further processing the raw materials, which can save costs and facilitate industrialization. In addition to oxygen, the reaction raw materials are at least one of oxides, carbonates, phosphates, and nitrates of the elements contained in the phosphor.
[0036] After the prepared raw materials are mixed, they are ground to make them uniform. The grinding can be carried out in an agate mortar or a ball mill. During the grinding process, alcohol or acetone solvent can be added to the raw materials to speed up the grinding process. The average particle size of the mixture obtained by grinding is preferably 200 mesh to 600 mesh, so that the raw materials in the mixture can fully react in the subsequent process.
[0037] Among them, in step 2), the sintering heating rate is 3-5°C / min, the pre-sintering (i.e., sintering I) temperature is 600°C-800°C, the holding time is 3-8 hours, and the secondary sintering (i.e., sintering II) temperature is 1200°C-1400°C, and the holding time is 3-8 hours.
[0038] In step 3), the particle size of the near-infrared phosphor obtained by grinding is not limited. Preferably, the sintered body is ground to a particle size of 80 mesh to 400 mesh.
[0039] In order to better understand the present invention, the phosphate near-infrared phosphor, preparation method and application in near-infrared LED light source of the present application are further described by specific examples. The raw materials used to prepare the phosphor in the following implementation cases are all commercially available (purity greater than 99%).
[0040] Embodiment 1:
[0041] When x=0.05, the chemical formula of the phosphate near-infrared phosphor is CdTi4(PO4)6:0.05Cr 3+ The preparation method of the phosphate near-infrared phosphor is as follows:
[0042] (1) According to the chemical formula CdTi4(PO4)6:0.05Cr 3+ , weigh CdO, TiO2, H6NO4P and Cr2O3 respectively, mix them thoroughly and grind them until they are uniform (particle size is 200 mesh to 600 mesh), put them into a corundum crucible, and then put them into a high-temperature box furnace, first pre-sinter them at 700℃ for 5 hours, wait for them to cool down to room temperature naturally, then take them out and grind them again to obtain a pre-sintered body.
[0043] (2) The pre-sintered body is then placed in a high temperature box furnace, heated to 1300°C and calcined for 5 hours. After the reaction is completed, the pre-sintered body is naturally cooled to room temperature to obtain a sintered body.
[0044] (3) The sintered body is fully ground again to a particle size of 80-400 meshes to obtain the desired near-infrared phosphor.
[0045] Embodiment 2:
[0046] When x=0.07, the chemical formula of the phosphate near-infrared phosphor is CdTi4(PO4)6:0.07Cr 3+ The preparation method of the phosphate near-infrared phosphor is as follows:
[0047] (1) According to the chemical formula CdTi4(PO4)6:0.07Cr 3+ , weigh CdO, TiO2, H6NO4P and Cr2O3 respectively, mix them thoroughly and grind them until they are uniform (particle size is 200 mesh to 600 mesh), put them into a corundum crucible, and then put them into a high-temperature box furnace, first pre-sinter them at 700℃ for 5 hours, wait for them to cool down to room temperature naturally, then take them out and grind them again to obtain a pre-sintered body.
[0048] (2) The pre-sintered body is then placed in a high temperature box furnace, heated to 1300°C and calcined for 5 hours. After the reaction is completed, the pre-sintered body is naturally cooled to room temperature to obtain a sintered body.
[0049] (3) The sintered body is fully ground again to a particle size of 80-400 meshes to obtain the desired near-infrared phosphor.
[0050] Embodiment 3:
[0051] When x=0.09, the chemical formula of the phosphate near-infrared phosphor is CdTi4(PO4)6:0.09Cr 3+ The preparation method of the phosphate near-infrared phosphor is as follows:
[0052] (1) According to the chemical formula CdTi4(PO4)6:0.09Cr 3+ , weigh CdO, TiO2, H6NO4P and Cr2O3 respectively, mix them thoroughly and grind them until they are uniform (particle size is 200 mesh to 600 mesh), put them into a corundum crucible, and then put them into a high-temperature box furnace, first pre-sinter them at 600℃ for 8 hours, wait for them to cool down naturally to room temperature, then take them out and grind them again to obtain a pre-sintered body.
[0053] (2) The pre-sintered body is then placed in a high temperature box furnace, heated to 1200°C and calcined for 8 hours. After the reaction is completed, the pre-sintered body is naturally cooled to room temperature to obtain a sintered body.
[0054] (3) The sintered body is fully ground again to a particle size of 80-400 meshes to obtain the desired near-infrared phosphor.
[0055] Embodiment 4:
[0056] When x=0.11, the chemical formula of the phosphate near-infrared phosphor is CdTi4(PO4)6:0.11Cr 3+ The preparation method of the phosphate near-infrared phosphor is as follows:
[0057] (1) According to the chemical formula CdTi4(PO4)6:0.11Cr 3+ , weigh CdO, TiO2, H6NO4P and Cr2O3 respectively, mix them thoroughly and grind them until they are uniform (particle size is 200 mesh to 600 mesh), put them into a corundum crucible, and then put them into a high-temperature box furnace, first pre-sinter them at 800℃ for 3 hours, wait for them to cool down naturally to room temperature, then take them out and grind them again to obtain a pre-sintered body.
[0058] (2) The pre-sintered body is then placed in a high temperature box furnace, heated to 1400°C and calcined for 3 hours. After the reaction is completed, the pre-sintered body is naturally cooled to room temperature to obtain a sintered body.
[0059] (3) The sintered body is fully ground again to a particle size of 80-400 meshes to obtain the desired near-infrared phosphor.
[0060] Embodiment 5:
[0061] When x=0.13, the chemical formula of the phosphate near-infrared phosphor is CdTi4(PO4)6:0.13Cr 3+ The preparation method of the phosphate near-infrared phosphor is as follows:
[0062] (1) According to the chemical formula CdTi4(PO4)6:0.13Cr 3+ , weigh CdO, TiO2, H6NO4P and Cr2O3 respectively, mix them thoroughly and grind them until they are uniform (particle size is 200 mesh to 600 mesh), put them into a corundum crucible, and then put them into a high-temperature box furnace, first pre-sinter them at 700℃ for 5 hours, wait for them to cool down to room temperature naturally, then take them out and grind them again to obtain a pre-sintered body.
[0063] (2) The pre-sintered body is then placed in a high temperature box furnace, heated to 1300°C and calcined for 5 hours. After the reaction is completed, the pre-sintered body is naturally cooled to room temperature to obtain a sintered body.
[0064] (3) The sintered body is fully ground again to a particle size of 80-400 meshes to obtain the desired near-infrared phosphor.
[0065] Test Characterization:
[0066] The XRD spectrum of the phosphate near-infrared phosphor prepared in Example 2 is as follows: Figure 1 The diffraction peaks in the figure correspond to CdTi4(PO4)6 and CdTi4(PO4)6:0.07Cr 3+ The typical diffraction peaks of , indicating that the obtained sample is pure phase.
[0067] The excitation spectrum of the phosphate near-infrared phosphor prepared in Example 2 is as follows: Figure 2 As shown, it shows that the excitation wavelength peaks are located at 343nm, 475nm, and 665nm.
[0068] The emission spectrum of the phosphate near-infrared phosphor prepared in Example 2 is as follows: Figure 3 As shown, it indicates that the emission wavelength peak is located at 835nm.
[0069] The temperature-dependent spectral intensity trend of the phosphate near-infrared phosphor prepared in Example 2 is as follows: Figure 4 shown.
[0070] The performance of the phosphate near-infrared phosphors prepared in the remaining examples is similar to that of Example 2.
[0071] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A Cr 3+ Phosphate-doped near-infrared phosphor, characterized in that: The chemical general formula of the near-infrared phosphor is CdTi4(PO4)6:xCr 3+ ; where x represents the mole fraction, and the value range of x is: 0 < x ≤ 0.2; the emission peak of the near-infrared phosphor is between 750 nm and 900 nm and can be excited by blue light.
2. The Cr according to claim 1 3+ Phosphate-doped near-infrared phosphor, characterized in that: The value range of x is: 0.05≤x≤0.
13.
3. The Cr according to claim 1 3+ Phosphate-doped near-infrared phosphor, characterized in that: The wavelength of the blue light is 450nm-480nm.
4. The Cr according to any one of claims 1 to 3 3+ The method for preparing phosphate-doped near-infrared phosphor is characterized in that: The following steps are involved: (1) sintering a mixture containing a Cd source, a Ti source, a Cr source, and a P source to obtain a sintered body; The Cd source is selected from at least one of Cd oxides and nitrates; the Cr source is selected from at least one of Cr oxides and Cr nitrates; the Ti source is selected from at least one of Ti oxides and Ti nitrates; the P source is selected from at least one of P oxides and P phosphates; (2) Grind the sintered body thoroughly to obtain.
5. The preparation method according to claim 4, characterized in that: The sintering in step (1) is specifically as follows: firstly sintering I is performed, cooling is performed to obtain a pre-sintered body, and then sintering II is performed to obtain a sintered body.
6. The preparation method according to claim 5, characterized in that: The sintering conditions of the sintering I are: temperature of 600° C. to 800° C. and time of 3 to 8 hours.
7. The preparation method according to claim 5, characterized in that: The conditions of sintering II are: temperature of 1200° C. to 1400° C. and time of 3 to 8 hours.
8. The preparation method according to claim 5, characterized in that: Before sintering I, the mixture is fully ground; the particle size of the ground mixture is 200-600 mesh; before sintering II, the pre-sintered body is fully ground.
9. The preparation method according to claim 4, characterized in that: In the step (2), the sintered body is ground to a particle size of 80-400 meshes.
10. Use of the near-infrared phosphor according to any one of claims 1 to 3 or the near-infrared phosphor prepared by the preparation method according to any one of claims 4 to 9 in preparing a near-infrared LED light source.
Citation Information
Patent Citations
Ultra-wideband near-infrared emission fluorescent powder and preparation method thereof
CN116120928A
Manganese-chromium-codoped alkaline earth titanium phosphate light-emitting thin film as well as preparation method and application thereof
CN103805189A
Luminescent material, preparation method thereof and LED light source