Target annealing method
By rotating annealing the target in an inert atmosphere, and using infrared cameras to monitor and adjust temperature differences in real time, the problem of difficult to ensure uniformity of the target grain size is solved, and a more uniform temperature heat and smaller average crystals are achieved The particle size improves the uniformity of the film layer and the coating rate.
Patent Information
- Application Number
- CN202411196107.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
In semiconductor chip production, the uniformity of the grain size of the target material is difficult to ensure, affecting the uniformity of the film layer and the coating rate. The existing annealing process cannot effectively control the uniformity of the target material's heating.
The target is rotated and annealed while rotating in an inert atmosphere. The infrared camera is used to monitor the surface temperature of the target in real time. By adjusting the heating power of the heating component, the absolute value of the temperature difference in different areas is within the range of 1 to 21°C to ensure temperature uniformity. This improves the uniformity of grain size.
Through rotary annealing and real-time temperature adjustment, the temperature uniformity of the target material and the uniformity of the grain size are significantly improved, local temperature differences are reduced, resulting in smaller average grain size, and improving the uniformity of the film layer and coating speed.
Smart Images

Figure CN119082422A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal processing, and in particular to a target material annealing method. Background Art
[0002] The most critical step in the production process of semiconductor chips is physical vapor deposition, and metal targets are one of the key consumables of physical vapor deposition. With the improvement of semiconductor processes, higher requirements are placed on the uniformity of film layers, and the coating rate determines the production cost, while the uniformity of the target grain size directly affects the uniformity of the film layer and the coating rate. The target material grows the grains by absorbing energy during annealing, and the annealing process directly affects the uniformity of the target grain size. Therefore, it is necessary to develop an annealing method that can ensure the uniformity of the target grain size. Summary of the invention
[0003] Based on the defects of the prior art, the purpose of the present application is to provide a target material annealing method to improve the uniformity of the target material grain size.
[0004] To achieve the above-mentioned purpose, the present application provides a target material annealing method, comprising the following steps: in an inert atmosphere, rotating the target material while performing annealing treatment, and then cooling the target material to obtain a target target material;
[0005] The equipment used for the annealing treatment has two or more heating components whose heating power can be independently controlled;
[0006] During the annealing process, an infrared camera is used to obtain the real-time temperature of the target surface, and according to the real-time temperature difference between different areas of the target, the heating power of each heating component is adjusted to control the maximum absolute value of the temperature difference between different areas of the target to be within the range of 1 to 21°C.
[0007] The above-mentioned target annealing method improves the uniformity of the target material's heat treatment by controlling the target material to rotate during the annealing process, thereby improving the uniformity of the target material's grain size; at the same time, an infrared camera is used to obtain the real-time temperature of the target material surface during the annealing process, and according to the difference between the real-time temperature value of different regions of the target material and the design temperature value, according to the real-time temperature difference of different regions of the target material, the heating power of the heating component is adjusted to control the maximum value of the absolute value of the temperature difference of different regions of the target material within the range of 1 to 21°C, such as 1°C, 3°C, 5°C, 8°C, 10°C, 12°C, 15°C, 18°C, 20°C, 21°C or any two of the above range values, to reduce the local temperature difference of the target material and improve its temperature uniformity, so that its grain size is more uniform and the average grain size is smaller. Preferably, the maximum value of the absolute value of the temperature difference of different regions of the target material is controlled within the range of 1 to 6°C to further improve the uniformity of the grain size and refine the average grain size.
[0008] Preferably, the infrared camera's photographing time interval is 28 to 122 seconds. By using the infrared camera's photographing time interval within the range of 28 to 122 seconds, such as 28s, 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, 110s, 120s, 122s or any two of the above ranges, the target material can have a good temperature uniformity during the annealing process with a relatively small number of photographs. More preferably, the infrared camera's photographing time interval is 28 to 40 seconds to further improve the uniformity of the grain size.
[0009] Preferably, the target material is at least one of aluminum, titanium, tantalum and copper.
[0010] Process parameters such as annealing temperature, annealing time, heating rate of annealing process, target rotation speed of annealing process will affect the uniformity of aluminum target grain size and average grain size.
[0011] Preferably, the target material is aluminum, and the design temperature program of the annealing treatment is as follows: heating to 100-500°C at a rate of 2-60°C / min and keeping warm for 14-610min; during the annealing treatment, the rotation speed of the target material is 1-120 revolutions / min to make the uniformity of the grain size of the aluminum target better and the average grain size smaller.
[0012] Preferably, the target material is titanium, and the design temperature program of the annealing treatment is as follows: heating to 300-1400°C at a rate of 2-60°C / min and keeping warm for 14-610min; during the annealing treatment, the rotation speed of the target material is 1-120 revolutions / min to make the titanium target grain size more uniform and the average grain size smaller.
[0013] Preferably, the target material is tantalum, and the design temperature program of the annealing treatment is as follows: heating to 400-1600°C at a rate of 1-60°C / min and keeping warm for 30-1000min; during the annealing treatment, the rotation speed of the target material is 0.5-120 turns / min, so as to make the tantalum target grain size more uniform and the average grain size smaller.
[0014] Preferably, the target material is copper, and the design temperature program of the annealing treatment is as follows: heating to 100-800°C at a rate of 1-60°C / min and keeping warm for 14-610min; during the annealing treatment, the rotation speed of the target material is 1-120 revolutions / min to make the copper target grain size more uniform and the average grain size smaller.
[0015] Preferably, the cooling method is liquid nitrogen cooling. Compared with natural cooling and other cooling methods, liquid nitrogen cooling is more conducive to improving the uniformity of the target grains and making the average grain size smaller.
[0016] Preferably, the annealing treatment equipment comprises a reaction chamber (1) and a rotating device (4), wherein the reaction chamber (1) is provided with an infrared camera (2), a heating platform (3) and two or more heating tubes (5) with independently controllable heating power, wherein each heating tube (5) is parallelly distributed on the lower surface of the reaction chamber (1), the inner reaction chamber (3) is arranged above the heating platform (3), the infrared camera (2) can photograph the upper surface of the target material on the heating platform (3), the rotating device (4) can rotate the heating platform (3), and the reaction chamber (1) is provided with a gas or liquid inlet (7). During the annealing process, the heating platform (3) is rotated by the rotating device (4), thereby rotating the target material placed thereon; the upper surface of the target material is photographed by the infrared camera (2) to obtain the real-time temperature of different areas on the upper surface of the target material; nitrogen and / or inert gas is introduced through the inlet (7) to obtain an inert atmosphere, or liquid nitrogen is introduced to cool the target material.
[0017] Preferably, the material of the heating platform (3) is quartz.
[0018] Preferably, the upper surface of the reaction chamber (1) is provided with heat-insulating cotton (6). By providing the heat-insulating cotton (6) on the upper surface of the reaction chamber (1), the fluctuation of the internal temperature can be reduced, so that the target material is heated more evenly during the annealing process.
[0019] Preferably, the target material is at least one of aluminum, titanium, tantalum and copper.
[0020] Preferably, the inert atmosphere is a nitrogen atmosphere. Compared with inert gases, nitrogen is cheap.
[0021] Compared with the prior art, the beneficial effect of the present application is that the present application controls the rotation of the target material during the annealing process and uses an infrared camera to obtain the real-time temperature values of different areas on the target material surface. According to the real-time temperature difference between different areas of the target material, the heating power of the heating component is adjusted to control the temperature difference between different areas of the target material within a specific range, thereby improving the uniformity of heating of the target material during the annealing process and improving its temperature uniformity, thereby making the grain size more uniform. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the structure of the equipment used for annealing in each embodiment and comparative examples 3 and 4, wherein 1-reaction chamber, 2-infrared camera, 3-heating table, 4-rotating device, 5-heating tube, 6-insulating cotton, 7-gas or liquid inlet, 8-target material;
[0023] Figure 2 This is a metallographic microscope photo of the target material obtained in Example 1;
[0024] Figure 3This is a metallographic microscope photo of the target material obtained in Example 11;
[0025] Figure 4 This is a metallographic microscope photograph of the target material obtained in Comparative Example 1. DETAILED DESCRIPTION
[0026] In order to better illustrate the purpose, technical scheme and advantages of the present application, the present application will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present application in detail, rather than to limit the present application. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. The experimental reagents and instruments involved in the implementation of the present application are all commonly used ordinary reagents and instruments unless otherwise specified.
[0027] The annealing equipment used in the following embodiments includes a reaction chamber 1 and a rotating device 4;
[0028] An infrared camera 2, a heating table 3 and more than two heating tubes 5 with independently controllable heating power are arranged inside the reaction chamber 1, wherein each heating tube 5 is distributed in parallel on the lower surface inside the reaction chamber 1, and the heating table 3 is arranged above each heating tube 5. The infrared camera 2 can photograph the upper surface of the target material in the inner reaction chamber 3, and the rotating device 4 can rotate the heating table 3 to rotate the target material 8 thereon. A gas or liquid inlet 7 is arranged on the outer reaction chamber 1 to introduce nitrogen or liquid nitrogen. The heating table 3 is a quartz cavity, and a heat preservation cotton 6 is arranged on the upper surface inside the reaction chamber 1.
[0029] Example 1
[0030] This embodiment provides a target material annealing method, which includes the following steps:
[0031] (1) Place the aluminum target on the heating table
[0032] The target is stably placed on the heating table 3 to ensure that the target does not shake up and down, wherein the target used is a pure aluminum target with a diameter of 200 mm, a thickness of 9 mm and a purity of 99.9995%;
[0033] (2) Setting parameters
[0034] On the control panel, set the heating rate to 6°C / min, the annealing temperature to 250°C, the annealing time to 30min, the rotation speed of the rotating device 4 to 60 rpm, turn on the infrared camera, set the maximum absolute value of the temperature difference between each area on the upper surface of the target to 5°C, and the infrared camera photo time interval to 30s. The computer follows the infrared camera to calculate the real-time temperature of each area on the upper surface of the target, and adjusts the power of the corresponding heating tube 5 according to the real-time temperature difference between each area on the upper surface of the target to adjust the temperature in real time, reduce local temperature differences, and improve temperature uniformity;
[0035] (3) Turn on heating and rotation
[0036] Press the heating button and the rotary button to pass N through the inlet 7 2 Gas protects the target to prevent oxidation;
[0037] (4) Shutdown and cooling
[0038] The machine was turned off, and liquid nitrogen was introduced through the inlet 7 to cool the target to room temperature (25° C., the same below), and the target was taken out.
[0039] Example 2
[0040] The difference from Example 1 is that in step (2), the maximum absolute value of the temperature difference between each area on the upper surface of the target material is set to 2°C.
[0041] Example 3
[0042] The difference from Example 1 is that in step (2), the maximum absolute value of the temperature difference between each area on the upper surface of the target material is set to 20°C.
[0043] Example 4
[0044] The difference from Example 1 is that in step (2), the photo taking time interval of the infrared camera is set to 70s.
[0045] Example 5
[0046] The difference from Example 1 is that in step (2), the photographing time interval of the infrared camera is set to 120 seconds.
[0047] Example 6
[0048] The difference from Example 1 is that in step (2), the heating rate is set to 2° C. / min, the annealing temperature is 100° C., the annealing time is 600 min, and the rotation speed of the rotating device 4 is 1 revolution / min.
[0049] Example 7
[0050] The difference from Example 1 is that in step (2), the heating rate is set to 60° C. / min, the annealing temperature is 500° C., the annealing time is 15 min, and the rotation speed of the rotating device 4 is 120 rpm.
[0051] Embodiments 8 to 10
[0052] The difference from Example 6 is that the annealing temperature is different, see Table 1 for details.
[0053] Embodiment 11
[0054] The difference from Example 1 is that in step (4), the machine is shut down and then cooled naturally to room temperature.
[0055] Example 12
[0056] The difference from Example 1 is that in step (4), after shutting down, the machine is cooled to room temperature in deionized water whose initial temperature is room temperature.
[0057] Examples 13 to 21
[0058] The difference from Example 1 is that the target material used and the heating rate, annealing temperature, annealing time and rotation speed of the rotating device 4 in step (2) are different, see Table 1 for details.
[0059] Comparative Example 1
[0060] This comparative example provides a target material annealing method, which comprises the following steps:
[0061] (1) Place the aluminum target in the muffle furnace
[0062] A pure aluminum target with a diameter of 200 mm, a thickness of 9 mm and a purity of 99.9995% is placed stably at the bottom of the muffle furnace, and the muffle furnace heating tubes are on the side walls and the top;
[0063] (2) Setting parameters
[0064] On the control panel, the heating rate is 6℃ / min, the annealing temperature is 250℃, and the annealing time is 30min;
[0065] (3) Turn on heating
[0066] Press the heat button;
[0067] (4) Shutdown and cooling
[0068] After the machine is turned off and the temperature naturally drops to 100°C, the target is taken out and placed in deionized water with an initial temperature of room temperature to cool.
[0069] Comparative Example 2
[0070] The difference from Example 1 is that in step (2), the rotation speed of the rotating device 4 is set to 0.
[0071] Comparative Example 3
[0072] The difference from Example 1 is that in step (2), the infrared camera is not turned on, the computer does not calculate the real-time temperature of each area on the target surface, and the power of the corresponding heating tube 5 is not adjusted according to the real-time temperature difference between the areas on the target surface; in step (4), the target is taken out and cooled in deionized water with an initial temperature of room temperature.
[0073] The average grain sizes of the targets of the above embodiments and comparative examples are shown in Table 1.
[0074] Table 1
[0075]
[0076]
[0077] From the above data, it can be seen that the target materials obtained in each embodiment of the present application have good grain uniformity and low average grain size, among which the average grain size of the aluminum target is below 275μm, the average grain size of the copper target is below 75μm, the average grain size of the titanium target is below 65μm, and the average grain size of the tantalum target is below 180μm. During the annealing process of Comparative Examples 1 to 3, the target material was not rotated and / or photographed to control the temperature difference in different areas, resulting in a low average grain size. By comparing Examples 1, 8 to 10, it can be seen that the annealing temperature will affect the average grain size of the target material. When the target material is aluminum, the annealing temperature is in the range of 150 to 250°C, and the average grain size of the target material is smaller. By comparing Examples 1, 11 to 12, it can be seen that the cooling method will affect the average grain size of the target material. When the target material is taken out and cooled with liquid nitrogen, the average grain size of the target material is smaller.
[0078] The grain size of the target material obtained in each embodiment and comparative example was observed using a metallographic microscope. Figure 2 and Figure 3 It can be seen that the target materials obtained in Examples 1 and 12 have good grain uniformity and no abnormally large grains. Figure 4 It can be seen that the target material obtained in Comparative Example 1 has a grain uniformity deviation and has abnormally large grains.
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A target annealing method, characterized in that: The following steps are involved: Under an inert atmosphere, the target material is annealed while being rotated, and then cooled to obtain a target target material; The equipment used for the annealing treatment has two or more heating components whose heating power can be independently controlled; During the annealing process, an infrared camera is used to obtain the real-time temperature of the target surface, and according to the real-time temperature difference between different areas of the target, the heating power of each heating component is adjusted to control the maximum absolute value of the temperature difference between different areas of the target to be within the range of 1 to 21°C.
2. The target annealing method according to claim 1, characterized in that: The maximum absolute value of the temperature difference between different areas of the target is controlled to be within the range of 1 to 6°C.
3. The target annealing method according to claim 1, characterized in that: The infrared camera takes pictures at a time interval of 28 to 122 seconds.
4. The target annealing method according to claim 3, characterized in that: The infrared camera takes pictures at a time interval of 28 to 40 seconds.
5. The target annealing method according to claim 1, characterized in that: The target material is at least one of aluminum, titanium, tantalum and copper.
6. The target annealing method according to claim 1, characterized in that: At least one of the following conditions is met: S1. The target material is aluminum, and the design temperature program of the annealing treatment is as follows: heating to 100-500°C at a rate of 2-60°C / min and keeping warm for 14-610min; during the annealing process, the rotation speed of the target material is 1-120 laps / min; S2. The target material is titanium, and the design temperature program of the annealing treatment is as follows: heating to 300-1400°C at a rate of 2-60°C / min and keeping warm for 14-610min; during the annealing process, the rotation speed of the target material is 1-120 laps / min; S3. The target material is tantalum, and the design temperature program of the annealing treatment is as follows: heating to 400-1600°C at a rate of 1-60°C / min and keeping warm for 30-1000min; during the annealing process, the rotation speed of the target is 0.5-120 laps / min; S4. The target material is copper, and the design temperature program of the annealing treatment is as follows: heating to 100-800°C at a rate of 1-60°C / min and keeping warm for 14-610min; during the annealing treatment, the rotation speed of the target material is 1-120 revolutions / min.
7. The target annealing method according to claim 1, characterized in that: The cooling method is liquid nitrogen cooling.
8. The target annealing method according to claim 1, characterized in that: The equipment used for annealing treatment comprises a reaction chamber (1) and a rotating device (4); an infrared camera (2), a heating platform (3) and two or more heating tubes (5) whose heating power can be independently controlled are arranged inside the reaction chamber (1); wherein each heating tube (5) is distributed in parallel on the lower surface inside the reaction chamber (1); the inner reaction chamber (3) is arranged above the heating platform (3); the infrared camera (2) can photograph the upper surface of the target material on the heating platform (3); the rotating device (4) can rotate the heating platform (3); and a gas or liquid inlet (7) is arranged on the reaction chamber (1).
9. The target annealing method according to claim 8, characterized in that: The material of the heating platform (3) is quartz; and / or The upper surface of the interior of the reaction chamber (1) is provided with heat-insulating cotton (6).
10. The target annealing method according to claim 1, characterized in that: The inert atmosphere is a nitrogen atmosphere.