Processing and manufacturing method of high-strength corrosion-resistant aluminum alloy
By adding nano Al2O3 ceramic particles to the aluminum alloy and performing multi-stage treatment, combined with the organic superhydrophobic surface treatment of silver nanoparticles, the problem of insufficient corrosion resistance of aluminum alloy in acid and alkali environment is solved, and its strength and resistance are significantly improved Corrosive performance, extends service life and realizes self-cleaning function.
Patent Information
- Application Number
- CN202411207809.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to significantly improve the corrosion resistance of aluminum alloys while ensuring the strength of the aluminum alloy. Especially in acid and alkali environments, stress corrosion and cracking problems are serious, which shortens the service life of the material.
By adding nano Al2O3 ceramic particles to the aluminum alloy and carrying out multi-stage solid solution and aging treatment, combined with silver nanoparticles organic superhydrophobic surface treatment, a high-strength corrosion-resistant aluminum alloy is formed. Specific steps include smelting, multi-stage solid solution, multi-stage aging, surface pretreatment and annealing, the addition of nano Al2O3 ceramic particles is 1.0% to 1.5%, and silver nanoparticle deposition and spraying treatment to improve surface corrosion resistance.
It significantly improves the mechanical properties, damage resistance and wear resistance of aluminum alloy, while enhancing its corrosion resistance in acid and alkali environments, extending its service life, and realizes self-cleaning function through the organic superhydrophobic surface of silver nanoparticles. .
Smart Images

Figure BDA0005019525290000061 
Figure BDA0005019525290000081
Abstract
Description
Technical Field
[0001] The invention relates to a processing and manufacturing method of a high-strength corrosion-resistant aluminum alloy, and belongs to the technical field of aluminum alloy manufacturing. Background Art
[0002] Aluminum is a widely used metal element in the modern industrial system, and its usage in metal materials is second only to steel. It has been widely used in aerospace, petrochemical, shipbuilding, energy and power and other fields. Although the passivation layer on the surface of light alloys can prevent corrosion reactions in the matrix, there is a risk of being destroyed in acidic and alkaline environments, especially when multiple factors such as corrosion and stress interact, stress corrosion cracking is very likely to occur, which greatly shortens the service life of light alloy materials.
[0003] At present, the technologies to improve the corrosion resistance of high-strength aluminum alloys include alloy composition optimization design, processing technology optimization and improvement, multi-stage aging, spraying corrosion-resistant coatings, etc. Changes in process and composition will improve the corrosion resistance of alloy materials to a certain extent, but will also reduce the mechanical properties of the materials to a certain extent, thereby reducing the service life. Therefore, how to efficiently and stably improve the corrosion resistance of aluminum alloys, extend the service life while ensuring strength, is a technical problem that needs to be solved urgently. Summary of the invention
[0004] In order to simultaneously improve the corrosion resistance and strength of aluminum alloys, the present invention provides a processing and manufacturing method for high-strength corrosion-resistant aluminum alloys, which specifically includes the following steps:
[0005] (1) Melting: After melting Al block, Al-Si alloy, Al-Cu alloy, Al-Fe alloy, Al-Mn alloy, Al-Sc alloy, Al-Mg alloy, and Al-Zr alloy, add nano-Al2O3 ceramic particles, stir evenly, remove excess impurities on the liquid surface, cast into aluminum ingots using a metal mold, and then roll them through multiple passes to obtain aluminum alloy plates; the amount of the nano-Al2O3 ceramic particles added is 1.0% to 1.5% of the total mass of the Al block, Al-Si alloy, Al-Cu alloy, Al-Fe alloy, Al-Mn alloy, Al-Sc alloy, Al-Mg alloy, and Al-Zr alloy.
[0006] (2) Multi-stage solution treatment: The aluminum alloy plate obtained in step (1) is heated to 435-465° C. and kept at this temperature for 6-12 hours to complete the first stage solution treatment; then the aluminum alloy plate is further heated to 470-495° C. and kept at this temperature for 2-6 hours, and immediately quenched.
[0007] (3) Multi-stage aging treatment: The aluminum alloy plate after quenching in step (2) is heated to 90-120°C, kept at this temperature for 2-6 hours, and then cooled to complete the first stage of low-temperature aging treatment; the cooled alloy is heated to 165-175°C, kept at this temperature for 14-18 hours, and then cooled to room temperature to obtain an aluminum alloy substrate.
[0008] (4) Surface pretreatment: The aluminum alloy substrate obtained in step (3) is cleaned in a solution mixture of acetone, ethanol and deionized water in an ultrasonic bath for 30 to 40 minutes and then dried to remove impurities (organic and inorganic) from the substrate surface.
[0009] (5) Preparation of silver nanoparticle organic super-hydrophobic surface: The aluminum alloy substrate treated in step (4) was vertically immersed in a nitric acid solution for etching, the etched plate was washed with deionized water and dried for a period of time, and after being deposited in a 5.5-6.5 mol / L silver nitrate solution in an open environment at 25° C. for 20-40 minutes, a stearic acid solution was sprayed onto the surface of the Ag-NP (silver nanoparticle) coated aluminum alloy plate using a spray gun machine at 23-28° C.
[0010] (6) Annealing: After the aluminum alloy plate obtained in step (5) is placed at room temperature for 6 hours, the aluminum alloy plate is annealed at 155-165° C. for 1 hour to obtain a high-strength, corrosion-resistant aluminum alloy.
[0011] Preferably, the high-strength corrosion-resistant aluminum alloy contains 2.0% to 2.5% Mg, 0.5% to 0.8% Si, 0.4% to 0.8% Fe, 0.3% to 0.4% Cu, 0.1% to 0.2% Zr, 0.1% to 0.2% Sc, and the rest are Al elements and other trace elements.
[0012] Preferably, in step (1), the aluminum ingot undergoes multi-stage rolling for no less than 20 times.
[0013] Preferably, the specific process of smelting in step (1) is: putting the weighed Al block into the bottom of a crucible preheated to dark red, and heating it to melt; when the Al block is completely melted, raising the temperature to 750°C, adding the preheated Al-Si alloy, and after the Al-Si alloy is completely melted, adding Al-Cu, Al-Fe, Al-Mn, Al-Sc, Al-Mg, and Al-Zr alloys and stirring evenly, and finally adding nano-Al2O3 ceramic particles and stirring evenly.
[0014] Preferably, the quenching medium in step (2) can be air, water or oil, and the temperature of the aluminum alloy plate drops to 39-42° C. after quenching.
[0015] Preferably, the heating rate of the solution treatment in step (2) is no more than 2°C / min.
[0016] Preferably, in step (5), the concentration of the nitric acid solution used for etching is 2 mol / L, and the etching time is 7 to 10 min; the concentration of the silver nitrate solution used for deposition is 5.5 to 6.5 mol / L, and the deposition time is 20 to 40 minutes.
[0017] Preferably, the concentration of the stearic acid solution in step (5) is 6.67 g / L, and the preparation method is to dissolve stearic acid in anhydrous ethanol.
[0018] Preferably, the spraying distance in step (5) is 12 to 14 cm.
[0019] Beneficial Effects of the Invention
[0020] (1) After the aluminum alloy is modified by adding non-metallic reinforcing phase nano-Al2O3 ceramic particles, the reinforcing phase itself has an extremely stable structure and hardness. It is dispersed in the aluminum alloy matrix and can effectively hinder the movement of matrix grains under stress, thereby improving the mechanical properties of the aluminum alloy matrix and playing a role in refining grains and improving the structure.
[0021] (2) Adding alloying elements Si, Zr, Mg and Cu to Al and undergoing two-stage solid solution aging treatment can produce a precipitation-strengthened aluminum alloy with low density, excellent mechanical properties and machinability, high strength and good ductility, which endows the alloy with excellent damage resistance and high durability. The addition of Sc causes discontinuity and coarsening of the precipitation phase at the grain boundary, and also promotes the uniform distribution of dispersed Al3 (Sc, Zr) phase particles, effectively hindering dislocation movement, and helping to improve the strength, hardness, elongation, fracture toughness and wear resistance of the aluminum alloy.
[0022] (3) The smooth organic super-hydrophobic surface composed of silver nanoparticles and stearic acid in the invention is fluorine-free, strong, naturally stable, and has excellent self-cleaning function and corrosion resistance.
[0023] (4) The organic hydrophobic surface of silver nanoparticles after annealing The finally obtained organic super-hydrophobic surface of silver nanoparticles shows a static water contact angle of 160±1° and a dynamic angle of 2°, which can effectively exclude liquid pollutants or dust pollution and protect the material. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is further described below by specific implementation methods. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0025] Example 1
[0026] A processing and manufacturing method for a high-strength corrosion-resistant aluminum alloy specifically comprises the following steps:
[0027] (1) A weighed Al block is placed at the bottom of a crucible preheated to dark red, and the temperature is raised to melt. When the Al block is completely melted, the temperature is raised to 750°C; a preheated Al-Si alloy is added, and after the Al-Si alloy is completely melted, Al-Cu alloy, Al-Fe alloy, Al-Mn alloy, Al-Sc alloy, Al-Mg alloy, and Al-Zr alloy are added and stirred evenly, and then nano-Al2O3 ceramic particles are added and stirred evenly; excess impurities on the liquid surface are removed, and an aluminum ingot is cast into an aluminum ingot using a metal mold, and then hot-rolled for 24 times to obtain an aluminum alloy plate, wherein the amount of the nano-Al2O3 ceramic particles added is 1.0% of the total mass of the Al block, the Al-Si alloy, the Al-Cu alloy, the Al-Fe alloy, the Al-Mn alloy, the Al-Sc alloy, the Al-Mg alloy, and the Al-Zr alloy.
[0028] (2) The aluminum alloy plate obtained in step (1) is heated to 445° C. and kept at this temperature for 8 h to complete the first stage of solid solution; then the alloy is further heated to 470° C. and kept at this temperature for 4 h to complete the second stage of solid solution, and immediately water quenched to reduce the temperature of the aluminum alloy plate to 40° C.
[0029] (3) The aluminum alloy quenched in step (2) is heated to 110° C., kept at this temperature for 2 h, and then air-cooled to complete the first stage of low-temperature aging treatment; the cooled alloy is heated to 165° C., kept at this temperature for 14 h, completed the second stage of low-temperature aging treatment, and then cooled to room temperature to obtain an aluminum alloy substrate.
[0030] (4) The aluminum alloy substrate obtained in step (3) is cleaned in a solution mixture of acetone, ethanol and deionized water in an ultrasonic bath for 35 minutes to remove impurities from the surface of the substrate.
[0031] (5) The aluminum alloy substrate treated in step (4) was vertically immersed in a 2 mol / L nitric acid solution for etching for 7 min, and then the etched plate was washed with deionized water and dried for a period of time, and then deposited in a 5.5 mol / L silver nitrate solution for 20 min in an open environment at 25°C, and stearic acid was fully dissolved in anhydrous ethanol at 40°C to prepare a 6.67 g / L stearic acid solution, and then the stearic acid solution was placed at room temperature for a few minutes and transferred to a spray gun, which was operated at 23°C and sprayed at an optimized distance of 12 cm. The solution was sprayed onto the surface of the Ag-NP-coated aluminum alloy plate. After spraying, the plate was placed at room temperature for 6 h.
[0032] (6) The aluminum alloy plate obtained in step (5) is placed in an oven and annealed at 155° C. for 1 hour. Finally, a silver nanoparticle organic super hydrophobic surface is formed on the substrate to obtain a high-strength, corrosion-resistant aluminum alloy.
[0033] The high-strength, corrosion-resistant aluminum alloy prepared in this embodiment contains 2.325% Mg, 0.568% Si, 0.74% Fe, 0.38% Cu, 0.106% Zr, 0.17% Sc, and the rest are Al elements and other trace elements.
[0034] Example 2
[0035] (1) A weighed Al block is placed at the bottom of a crucible preheated to dark red, and the temperature is raised to melt. When the Al block is completely melted, the temperature is raised to 750°C; a preheated Al-Si alloy is added, and after the Al-Si alloy is completely melted, Al-Cu alloy, Al-Fe alloy, Al-Mn alloy, Al-Sc alloy, Al-Mg alloy, and Al-Zr alloy are added and stirred evenly, and then nano-Al2O3 ceramic particles are added and stirred evenly; excess impurities on the liquid surface are removed, and an aluminum ingot is cast into an aluminum ingot using a metal mold, and then hot-rolled for 20 times to obtain an aluminum alloy plate, wherein the amount of the nano-Al2O3 ceramic particles added is 1.25% of the total mass of the Al block, the Al-Si alloy, the Al-Cu alloy, the Al-Fe alloy, the Al-Mn alloy, the Al-Sc alloy, the Al-Mg alloy, and the Al-Zr alloy.
[0036] (2) heating the aluminum alloy plate obtained in step (1) to 445° C. and keeping the temperature for 6 hours to complete the first stage of solid solution; then further heating the alloy to 480° C. and keeping the temperature for 2 hours to complete the second stage of solid solution, and immediately oil quenching to reduce the temperature of the aluminum alloy plate to 40° C.;
[0037] (3) The aluminum alloy quenched in step (2) is heated to 100° C., kept at this temperature for 4 hours, and then air-cooled to complete the first stage of low-temperature aging treatment; the cooled alloy is heated to 170° C., kept at this temperature for 16 hours to complete the second stage of low-temperature aging treatment, and then cooled to room temperature to obtain an aluminum alloy substrate.
[0038] (4) The aluminum alloy substrate obtained in step (3) is cleaned in a solution mixture of acetone, ethanol and deionized water in an ultrasonic bath for 40 minutes to remove impurities from the surface of the substrate.
[0039] (5) The aluminum alloy substrate treated in step (4) was vertically immersed in a 2 mol / L nitric acid solution for etching for 8 min, and then the etched plate was washed with deionized water and dried for a period of time, and then deposited in a 6.0 mol / L silver nitrate solution for 30 min in an open environment at 25°C, and stearic acid was fully dissolved in anhydrous ethanol at 40°C to prepare a 6.67 g / L stearic acid solution, and then the stearic acid solution was placed at room temperature for a few minutes and transferred to a spray gun, which was operated at 25°C and sprayed at an optimized distance of 13 cm. The solution was sprayed onto the surface of the Ag-NP-coated aluminum alloy plate. After spraying, the plate was placed at room temperature for 6 h.
[0040] (6) The aluminum alloy plate obtained in step (5) is placed in an oven and annealed at 160° C. for 1 hour. Finally, a silver nanoparticle organic super hydrophobic surface is formed on the substrate to obtain a high-strength, corrosion-resistant aluminum alloy.
[0041] The high-strength, corrosion-resistant aluminum alloy prepared in this embodiment contains 2.37% Mg, 0.76% Si, 0.82% Fe, 0.326% Cu, 0.14% Zr, 0.128% Sc, and the rest are Al elements and other trace elements.
[0042] Example 3
[0043] (1) A weighed Al block is placed at the bottom of a crucible preheated to dark red, and the temperature is raised to melt. When the Al block is completely melted, the temperature is raised to 750°C; a preheated Al-Si alloy is added, and after the Al-Si alloy is completely melted, Al-Cu alloy, Al-Fe alloy, Al-Mn alloy, Al-Sc alloy, Al-Mg alloy, and Al-Zr alloy are added and stirred evenly, and then nano-Al2O3 ceramic particles are added and stirred evenly; excess impurities on the liquid surface are removed, and an aluminum ingot is cast into an aluminum ingot using a metal mold, and then hot-rolled for 20 times to obtain an aluminum alloy plate, wherein the amount of the nano-Al2O3 ceramic particles added is 1.5% of the total mass of the Al block, the Al-Si alloy, the Al-Cu alloy, the Al-Fe alloy, the Al-Mn alloy, the Al-Sc alloy, the Al-Mg alloy, and the Al-Zr alloy.
[0044] (2) heating the aluminum alloy plate obtained in step (1) to 445° C. and keeping the temperature for 6 hours to complete the first stage of solid solution; then further heating the alloy to 480° C. and keeping the temperature for 2 hours to complete the second stage of solid solution, and immediately oil quenching to reduce the temperature of the aluminum alloy plate to 40° C.;
[0045] (3) The aluminum alloy quenched in step (2) is heated to 100° C., kept at this temperature for 4 hours, and then air-cooled to complete the first stage of low-temperature aging treatment; the cooled alloy is heated to 170° C., kept at this temperature for 16 hours to complete the second stage of low-temperature aging treatment, and then cooled to room temperature to obtain an aluminum alloy substrate.
[0046] (4) The aluminum alloy substrate obtained in step (3) is cleaned in a solution mixture of acetone, ethanol and deionized water in an ultrasonic bath for 30 minutes to remove impurities from the surface of the substrate.
[0047] (5) The aluminum alloy substrate treated in step (4) was vertically immersed in a 2 mol / L nitric acid solution for etching for 10 min, and then the etched plate was washed with deionized water and dried for a period of time, and then deposited in a 6.5 mol / L silver nitrate solution for 40 min in an open environment at 25°C, and stearic acid was fully dissolved in anhydrous ethanol at 40°C to prepare a 6.67 g / L stearic acid solution, and then the stearic acid solution was placed at room temperature for a few minutes and transferred to a spray gun, which was operated at 24°C and sprayed at an optimized distance of 14 cm. The solution was sprayed onto the surface of the Ag-NP-coated aluminum alloy plate. After spraying, the plate was placed at room temperature for 6 h.
[0048] (6) The aluminum alloy plate obtained in step (5) is placed in an oven and annealed at 165° C. for 1 hour. Finally, a silver nanoparticle organic super hydrophobic surface is formed on the substrate to obtain a high-strength, corrosion-resistant aluminum alloy.
[0049] The high-strength, corrosion-resistant aluminum alloy prepared in this embodiment contains 2.45% Mg, 0.63% Si, 0.59% Fe, 0.33% Cu, 0.151% Zr, 0.13% Sc, and the rest are Al elements and other trace elements.
[0050] Comparative Example
[0051] The comparative example was set up with reference to Example 1. Except for special instructions in the table, the other conditions were the same as those in Example 1. As shown in Table 1.
[0052] Table 1 Technical differences between comparative examples 1 to 5 and example 1 in the preparation process
[0053]
[0054] Performance evaluation:
[0055] (1) Corrosion resistance test
[0056] The aluminum alloys obtained in Examples 1-3 of the present invention and the aluminum alloys obtained in Comparative Examples 1-5 were prepared into aluminum alloy blocks of 10 mm×10 mm×10 mm, respectively, and then electrochemical experiments were performed. A three-electrode system was used, with the auxiliary electrode being a platinum electrode, the reference electrode being a saturated calomel electrode, the sample to be tested being the research electrode, and the test medium being a 3% NaCl aqueous solution. The test temperature was carried out at room temperature, and the exposed area in the solution was 1 cm 2 . Self-corrosion potential E0 (V) and self-corrosion current I0 (A / cm 2 ). The test results are shown in Table 2.
[0057] Table 2 Test results of aluminum alloy self-corrosion potential and self-corrosion current obtained in all embodiments and comparative examples
[0058] Sample No. <![CDATA[E0(V)]]> <![CDATA[I0(A / cm 2 )]]> Example 1 -1.025 <![CDATA[2.254X10 -8 ]]> Example 2 -1.007 <![CDATA[2.543X10 -8 ]]> Example 3 -0.948 <![CDATA[1.368X10 -9 ]]> Comparative Example 1 -1.387 <![CDATA[3.196X10 -7 ]]> Comparative Example 2 -1.721 <![CDATA[9.296X10 -6 ]]> Comparative Example 3 -1.538 <![CDATA[7.384X10 -5 ]]> Comparative Example 4 -1.965 <![CDATA[6.223X10 -6 ]]> Comparative Example 5 -3.358 <![CDATA[3.472X10 -4 ]]>
[0059] (1) Corrosion resistance and mechanical properties test
[0060] The corrosion resistance and mechanical properties of the aluminum alloy materials of Examples 1-3 of the present invention and Comparative Examples 1-5 were further tested according to the national standard GB / T6892-2006, and the test result codes and grades of the samples were visually evaluated according to Table 3. The test results are shown in Table 3, and the corrosion grade description is shown in Table 4.
[0061] Table 3 Corrosion grade and tensile strength test results of all embodiments and comparative examples
[0062] Sample No. Corrosion level Tensile strength / MPa Example 1 N 338.72 Example 2 N 332.9 Example 3 N 325.8 Comparative Example 1 EA 278.8 Comparative Example 2 EA 276.7 Comparative Example 3 EC 286.2 Comparative Example 4 EB 284.4
[0063] Table 4 Corrosion grade description
[0064]
[0065] In the three-electrode system, the corrosion potential represents the tendency of the material to corrode. The more negative the potential, the greater the tendency of the material to corrode. The corrosion current represents the corrosion rate of the material when corrosion occurs. The larger the corrosion current, the faster the material corrodes. The corrosion voltage of the embodiment of the present invention is greater than that of the comparative example, and the corrosion current is less than that of the comparative example, which can indicate that the aluminum alloy of the embodiment of the present invention has good corrosion resistance.
[0066] The corrosion resistance and strength of Comparative Example 1 in which nano ceramic particles, Zr and Sc elements are not added to the substrate are decreased. Nano ceramic particles, Zr and Sc can all produce strengthening effects in the matrix. And Sc and Zr also play an important role in improving the performance of the refined material organization. Comparative Example 3 in which the silver nanoparticle organic super hydrophobic layer is not prepared on the surface, has a significant decrease in corrosion performance, and the silver nanoparticle organic hydrophobic layer plays a positive role in improving the corrosion resistance of the substrate. The bonding strength between the silver nanoparticle organic hydrophobic layer and the substrate is affected, and the corrosion resistance of Comparative Example 4 without pretreatment on the surface is also decreased, and the surface layer is peeled off after corrosion, indicating that surface pretreatment has a positive effect on the combination of the silver nanoparticle organic super hydrophobic layer and the substrate. The corrosion resistance of the original aluminum alloy embodiment 5 is the worst among all sample aluminum alloys.
[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for processing and manufacturing a high-strength, corrosion-resistant aluminum alloy, characterized in that: The specific steps include: (1) Melting: After melting Al block, Al-Si alloy, Al-Cu alloy, Al-Fe alloy, Al-Mn alloy, Al-Sc alloy, Al-Mg alloy, and Al-Zr alloy, add nano-Al2O3 ceramic particles, stir evenly, remove excess impurities on the liquid surface, cast into aluminum ingots using a metal mold, and then roll them through multiple passes to obtain aluminum alloy plates; the amount of the nano-Al2O3 ceramic particles added is 1.0% to 1.5% of the total mass of the Al block, Al-Si alloy, Al-Cu alloy, Al-Fe alloy, Al-Mn alloy, Al-Sc alloy, Al-Mg alloy, and Al-Zr alloy; (2) Multi-stage solution treatment: heating the aluminum alloy plate obtained in step (1) to 435-465° C. and keeping the temperature for 6-12 hours to complete the first stage solution treatment; then further heating the aluminum alloy plate to 470-495° C. and keeping the temperature for 2-6 hours to complete the second stage solution treatment, and immediately quenching; (3) multi-stage aging treatment: heating the aluminum alloy plate after quenching in step (2) to 90-120° C., keeping the temperature for 2-6 hours, and then cooling the plate to complete the first stage of low-temperature aging treatment; heating the cooled alloy to 165-175° C., keeping the temperature for 14-18 hours, and then cooling the plate to complete the second stage of low-temperature aging treatment, thereby obtaining an aluminum alloy substrate; (4) Surface pretreatment: the aluminum alloy substrate obtained in step (3) is cleaned in a solution mixture of acetone, ethanol and deionized water in an ultrasonic bath for 30 to 40 minutes and then dried; (5) Preparing a silver nanoparticle organic super-hydrophobic surface: vertically immersing the aluminum alloy substrate treated in step (4) in a nitric acid solution for etching, washing the etched plate with deionized water and drying it for a period of time, depositing it in a 5.5-6.5 mol / L silver nitrate solution in an open environment at 25° C. for 20-40 minutes, spraying a stearic acid solution onto the surface of the silver nanoparticle-coated aluminum alloy plate at 23-28° C. using a spray gun machine, and leaving it at room temperature after spraying; (6) Annealing: The aluminum alloy plate obtained in step (5) is annealed at 155-165° C. for 1 h to obtain a high-strength, corrosion-resistant aluminum alloy.
2. The processing and manufacturing process of a high-strength corrosion-resistant aluminum alloy according to claim 1 is characterized in that: The high-strength corrosion-resistant aluminum alloy contains 2.0% to 2.5% Mg, 0.5% to 0.8% Si, 0.4% to 0.8% Fe, 0.3% to 0.4% Cu, 0.1% to 0.2% Zr, 0.1% to 0.2% Sc by mass percentage, and the rest are Al elements and other trace elements.
3. The processing and manufacturing process of a high-strength corrosion-resistant aluminum alloy according to claim 1 is characterized in that: In step (1), the aluminum ingot undergoes multi-stage rolling for no less than 20 times.
4. The processing and manufacturing process of a high-strength corrosion-resistant aluminum alloy according to claim 1 is characterized in that: The specific process of smelting in step (1) is as follows: a weighed Al block is placed at the bottom of a crucible preheated to dark red, and the temperature is raised to melt; when the Al block is completely melted, the temperature is raised to 750°C, and the preheated Al-Si alloy is added; after the Al-Si alloy is completely melted, Al-Cu, Al-Fe, Al-Mn, Al-Sc, Al-Mg, and Al-Zr alloys are added and stirred evenly; finally, nano-Al2O3 ceramic particles are added and stirred evenly.
5. The processing and manufacturing process of a high-strength corrosion-resistant aluminum alloy according to claim 1 is characterized in that: In step (2), the quenching medium can be air, water or oil. After quenching, the temperature of the aluminum alloy plate drops to 39-42°C.
6. The processing and manufacturing process of a high-strength corrosion-resistant aluminum alloy according to claim 1, characterized in that: The heating rate of the solution treatment in step (2) is not greater than 2°C / min.
7. The processing and manufacturing process of a high-strength corrosion-resistant aluminum alloy according to claim 1 is characterized in that: In step (5), the concentration of the nitric acid solution used for etching is 2 mol / L, and the etching time is 7 to 10 min; the concentration of the silver nitrate solution used for deposition is 5.5 to 6.5 mol / L, and the deposition time is 20 to 40 minutes.
8. The manufacturing process of a high-strength corrosion-resistant aluminum alloy according to claim 1, characterized in that: The concentration of the stearic acid solution in step (5) is 6.67 g / L, and the preparation method is to dissolve stearic acid in anhydrous ethanol.
9. The processing and manufacturing process of a high-strength corrosion-resistant aluminum alloy according to claim 1, characterized in that: The spraying distance of step (5) is 12 to 14 cm.