Anti-erosion copper-nickel-iron alloy and preparation method thereof

By adding nickel, iron, manganese, trace rare earth elements yttrium and nitrogen to the copper alloy, the process flow is optimized to form a dense corrosion product layer and hardened phase, the problem of insufficient corrosion resistance of copper alloy in seawater is solved, and high Significant improvements in mechanical properties and corrosion resistance.

CN119082543APending Publication Date: 2024-12-06ZHEJIANG WINJOY NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411001192.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing copper alloys are difficult to use in seawater for a long time, and although the addition of some elements can improve corrosion resistance, this often leads to a decrease in mechanical properties, limiting its application.

Method used

By adding nickel, iron, manganese, trace rare earth elements yttrium (Ce) and nitrogen (Nb) to the alloy, the chemical composition and process flow are optimized, and a erosion-resistant copper-nickel-ferroalloy is prepared, including Ni: 4.0-11.0%, Fe, : 1.0-2.0%, Mn: 0.2-1.0%, Ce: 0.02-0.05%, Nb: 0.005-0.025% and balance of copper, smelting, horizontal continuous casting, initial rolling, ring annealing, pre-finished product rolling , continuous annealing and stress-relieving annealing processes to form dense corrosion product layers and hardened phases, improving the mechanical and corrosion resistance of the alloy.

Benefits of technology

The alloy has achieved excellent mechanical properties and corrosion resistance, with tensile strength ≥400MPa, yield strength ≥330MPa, hardness ≥130HV, elongation A50≥8.0%, and no obvious corrosion on the surface after the 8h salt spray test, which significantly improved the use life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082543A_ABST
    Figure CN119082543A_ABST
Patent Text Reader

Abstract

The invention provides an anti-erosion copper-nickel-iron alloy and a preparation method thereof, and belongs to the technical field of copper alloy manufacturing. The nickel is added into the alloy, so that the effects of enhancing the hardness, improving the corrosion resistance and prolonging the service life can be achieved; the Fe element and the Mn element are added, so that a synergistic effect can be achieved, and the corrosion resistance of the alloy is greatly improved; by adding the trace alloy element Ce, a dense rare earth phase CeNi5 corrosion product layer can be formed with the Ni element in the alloy, microcracks are reduced, the alloy is firmly combined with a matrix, the corrosion rate can be effectively slowed down, and the corrosion resistance of the alloy is improved; by adding the Nb element, the high-temperature plasticity of the alloy can be remarkably improved, and meanwhile, the formed Ni3Nb compound can improve the hardening capacity of the alloy, so that the mechanical property of the alloy is improved; by optimizing the doping amount of the elements in the alloy, the mechanical property and the corrosion resistance of the alloy can be further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper alloy manufacturing, and in particular to a corrosion-resistant copper-nickel-iron alloy and a preparation method thereof. Background Art

[0002] Pure copper has excellent electrical conductivity, thermal conductivity, ductility and corrosion resistance. It is mainly used to make electrical equipment such as generators, busbars, cables, switchgear, transformers, and heat exchangers, pipelines, flat collectors for solar heating devices and other heat-conducting equipment. However, with the development of science and technology, the requirements for copper performance are getting higher and higher. Pure copper can no longer meet the technical requirements, so copper alloys have been developed on a large scale. Copper alloys are alloys composed of pure copper as a matrix and one or more other elements, including brass with zinc as the main alloying element, white copper with nickel as the main additive element, and bronze with tin as the main additive element.

[0003] Copper alloys are widely used in the fields of ships and marine engineering due to their good corrosion resistance and high corrosion resistance in polluted seawater and river water. Since seawater contains a large amount of corrosive chloride ions, it has a long-term corrosive effect on copper alloys. Even copper alloys are difficult to use in ships for a long time and require frequent maintenance. Although the corrosion resistance of copper alloys can be improved by adding some elements to them, the addition of these elements often leads to a decrease in the mechanical properties of copper alloys, which in turn limits the application of corrosion-resistant copper alloys.

[0004] Therefore, how to improve the corrosion resistance of copper alloys while ensuring their excellent mechanical properties has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0005] The object of the present invention is to provide a corrosion-resistant copper-nickel-iron alloy and a preparation method thereof. The corrosion-resistant copper-nickel-iron alloy provided by the present invention has excellent mechanical properties and corrosion resistance and can well resist seawater erosion.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides a corrosion-resistant copper-nickel-iron alloy, which comprises the following chemical components by mass percentage: Ni: 4.0-11.0%, Fe: 1.0-2.0%, Mn: 0.2-1.0%, Ce: 0.02-0.05%, Nb: 0.005-0.025% and the balance of copper.

[0008] Preferably, the corrosion-resistant copper-nickel-iron alloy comprises the following chemical components by mass percentage: Ni: 7.0-11.0%, Fe: 1.1-1.9%, Mn: 0.2-0.9%, Ce: 0.03-0.05%, Nb: 0.01-0.02% and the balance copper.

[0009] Preferably, the corrosion-resistant copper-nickel-iron alloy comprises the following chemical components by mass percentage: Ni: 9.0-11.0%, Fe: 1.2-1.9%, Mn: 0.22-0.85%, Ce: 0.04%, Nb: 0.02% and the balance of copper.

[0010] The present invention provides a method for preparing the corrosion-resistant copper-nickel-iron alloy described in the above technical solution, comprising the following steps:

[0011] (1) mixing alloy raw materials, sequentially melting and horizontally continuously casting to obtain alloy ingots;

[0012] (2) performing initial rolling on the alloy ingot obtained in step (1) to obtain an initial rolled alloy;

[0013] (3) subjecting the initially rolled alloy obtained in step (2) to coil annealing and pre-finished product rolling in sequence to obtain a rolled alloy;

[0014] (4) continuously annealing the rolled alloy obtained in step (3) to obtain an annealed alloy;

[0015] (5) The annealed alloy obtained in step (4) is subjected to finished product rolling and stress relief annealing in sequence to obtain a corrosion-resistant copper-nickel-iron alloy.

[0016] Preferably, in the step (1), the temperature of the horizontal continuous casting is 1190-1210° C., and the moving speed of the horizontal continuous casting is 110-130 mm / min.

[0017] Preferably, in the step (3), the holding temperature for the ring material annealing is 720-760° C., and the holding time for the ring material annealing is 12-16 hours.

[0018] Preferably, the total processing rate of the pre-finished product rolling in step (3) is 50-70%, and the number of passes of the pre-finished product rolling is 4-10 times.

[0019] Preferably, the temperature of the continuous annealing in the step (4) is 820-850° C., and the moving speed of the continuous annealing is 6-18 m / min.

[0020] Preferably, the total processing rate of the finished product rolling in step (5) is 15-40%, and the number of passes of the finished product rolling is 2-4 times.

[0021] Preferably, the temperature of the stress relief annealing in step (5) is 380-450°C.

[0022] The present invention provides a corrosion-resistant copper-nickel-iron alloy, which comprises the following chemical components by mass percentage: Ni: 4.0-11.0%, Fe: 1.0-2.0%, Mn: 0.2-1.0%, Ce: 0.02-0.05%, Nb: 0.005-0.025% and the balance of copper. The present invention can enhance hardness, improve corrosion resistance and prolong service life by adding nickel in the alloy; the addition of Fe element and Mn element can play a synergistic role and greatly improve the corrosion resistance of the alloy; by adding a trace alloy element Ce, a dense rare earth phase CeNi5 corrosion product layer can be formed with Ni element in the alloy, microcracks can be reduced, and the CeNi5 can be firmly combined with the matrix, which can effectively slow down the corrosion rate and improve the corrosion resistance of the alloy; the addition of Nb element can significantly improve the high-temperature plasticity of the alloy, and the Ni3Nb compound formed at the same time can improve the hardening ability of the alloy, thereby improving the mechanical properties of the alloy; by optimizing the doping amount of elements in the alloy, the mechanical properties and corrosion resistance of the alloy can be further improved. The results of the examples show that the corrosion-resistant copper-nickel-iron alloy provided by the present invention has a tensile strength of ≥400 MPa, a yield strength of ≥330 MPa, a hardness of ≥130 HV, and an elongation of A 50 ≥8.0%, excellent mechanical properties, at the same time, after 8h salt spray test, the alloy surface is bright and has no obvious corrosion, and has excellent corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a physical picture of the corrosion-resistant copper-nickel-iron alloy provided in Example 1 undergoing an 8-hour salt spray test. DETAILED DESCRIPTION

[0024] The invention provides a corrosion-resistant copper-nickel-iron alloy, which comprises the following chemical components by mass percentage: Ni: 4.0-11.0%, Fe: 1.0-2.0%, Mn: 0.2-1.0%, Ce: 0.02-0.05%, Nb: 0.005-0.025% and the balance of copper.

[0025] The corrosion-resistant copper-nickel-iron alloy provided by the present invention includes Ni: 4.0-11.0%, preferably 5.0-10.0%, and more preferably 6.0-8.0%, by mass percentage. In the present invention, nickel in the alloy can play a role in enhancing hardness, improving corrosion resistance and extending service life; by controlling the addition amount of Ni element, it can be avoided that too little addition leads to an insignificant strengthening effect on the alloy, and too much addition leads to excessively high cost of the copper alloy.

[0026] The corrosion-resistant copper-nickel-iron alloy provided by the present invention comprises Fe: 1.0-2.0%, preferably 1.2-1.8%, more preferably 1.4-1.6%, by mass percentage. In the present invention, the addition of Fe element can greatly improve the corrosion resistance of the alloy.

[0027] The corrosion-resistant copper-nickel-iron alloy provided by the present invention includes Mn in an amount of 0.2-1.0%, preferably 0.4-0.8%, and more preferably 0.6%, by mass percentage. In the present invention, the addition of Mn element can greatly improve the corrosion resistance of the alloy, and can also play a synergistic role with Fe element to further improve the corrosion resistance.

[0028] The corrosion-resistant copper-nickel-iron alloy provided by the present invention includes Ce: 0.02-0.05%, preferably 0.04%, by mass percentage. By adding a trace alloy element Ce, the present invention can form a dense rare earth phase CeNi5 corrosion product layer with Ni element in the alloy, reduce microcracks, and firmly bond with the matrix, which can effectively slow down the corrosion rate and improve the corrosion resistance of the alloy.

[0029] The corrosion-resistant copper-nickel-iron alloy provided by the present invention includes Nb: 0.005-0.025%, preferably 0.02%, by mass percentage. The present invention can significantly improve the high-temperature plasticity of the alloy by adding the Nb element, and the Ni3Nb compound formed can improve the hardening ability of the alloy, thereby improving the mechanical properties of the alloy.

[0030] The corrosion resistant copper-nickel-iron alloy provided by the present invention includes a balance of copper in terms of mass percentage. In the present invention, the copper is a matrix element of the alloy.

[0031] The invention can enhance the hardness, improve the corrosion resistance and prolong the service life of the alloy by adding nickel; the addition of Fe element and Mn element can play a synergistic role and greatly improve the corrosion resistance of the alloy; by adding a trace alloy element Ce, a dense corrosion product layer of rare earth phase CeNi5 can be formed in the alloy with Ni element, microcracks are reduced, and the CeNi5 layer is firmly bonded to the matrix, which can effectively slow down the corrosion rate and improve the corrosion resistance of the alloy; the addition of Nb element can significantly improve the high-temperature plasticity of the alloy, and the Ni3Nb compound formed can improve the hardening ability of the alloy, thereby improving the mechanical properties of the alloy; by optimizing the doping amount of the elements in the alloy, the mechanical properties and corrosion resistance of the alloy can be further improved.

[0032] The present invention also provides a method for preparing the corrosion-resistant copper-nickel-iron alloy described in the above technical solution, comprising the following steps:

[0033] (1) mixing alloy raw materials, sequentially melting and horizontally continuously casting to obtain alloy ingots;

[0034] (2) performing initial rolling on the alloy ingot obtained in step (1) to obtain an initial rolled alloy;

[0035] (3) subjecting the initially rolled alloy obtained in step (2) to coil annealing and pre-finished product rolling in sequence to obtain a rolled alloy;

[0036] (4) continuously annealing the rolled alloy obtained in step (3) to obtain an annealed alloy;

[0037] (5) The annealed alloy obtained in step (4) is subjected to finished product rolling and stress relief annealing in sequence to obtain a corrosion-resistant copper-nickel-iron alloy.

[0038] The invention mixes alloy raw materials, performs smelting and horizontal continuous casting in sequence, and obtains alloy ingots.

[0039] The present invention has no special limitation on the specific source and type of the alloy raw material, as long as the chemical composition of the corrosion-resistant copper-nickel-iron alloy meets the requirements.

[0040] The present invention has no special limitation on the process parameters of the smelting, which can be determined according to the technical common sense of those skilled in the art.

[0041] In the present invention, the temperature of the horizontal continuous casting is preferably 1190-1210°C, more preferably 1200°C; the moving speed of the horizontal continuous casting is preferably 110-130 mm / min, more preferably 120 mm / min. The present invention adopts the process of horizontal continuous casting to replace the existing semi-continuous casting, and controls its process parameters, which can not only avoid the enrichment in the alloy caused by too low temperature, affecting the elongation and bending of the finished product, but also avoid the difficulty in cooling and easy leakage into copper liquid caused by too high temperature, while also taking into account the grain size and the surface defects such as no broken crystals, cracks and ribs.

[0042] After the horizontal continuous casting is completed, the present invention preferably performs milling on the product of the horizontal continuous casting to obtain an alloy ingot. The present invention has no special limitation on the thickness of the milled surface, which can be determined according to the technical common sense of those skilled in the art.

[0043] After obtaining the alloy ingot, the alloy ingot is subjected to initial rolling to obtain an initial rolled alloy.

[0044] In the present invention, the total processing rate of the initial rolling is preferably 75-90%, more preferably 80-85%; the number of processing passes of the initial rolling is preferably 8-12, more preferably 10. The present invention can, through the initial rolling, on the one hand, cause a large deformation of the alloy ingot, thereby crushing the coarse grains inside the ingot and eliminating casting defects, and on the other hand, reduce the size of the alloy ingot.

[0045] After obtaining the initially rolled alloy, the present invention sequentially performs coil annealing and pre-product rolling on the initially rolled alloy to obtain a rolled alloy.

[0046] In the present invention, the holding temperature of the ring annealing is preferably 720-760°C, more preferably 730-750°C; the holding time of the ring annealing is preferably 12-16h, more preferably 13-15h, and further preferably 14h. The present invention can control the grain size of the alloy to 0.035-0.05*100 times by controlling the process parameters of the ring annealing, and the microstructure has no segregation.

[0047] In the present invention, the total processing rate of the pre-product rolling is preferably 50-70%, more preferably 55-65%, and further preferably 60%; the number of passes of the pre-product rolling is preferably 4-10. The present invention can reduce the size of the alloy and further refine the grain structure through pre-product rolling.

[0048] After the rolled alloy is obtained, the present invention performs continuous annealing on the rolled alloy to obtain the annealed alloy.

[0049] In the present invention, the temperature of the continuous annealing is preferably 820-850°C, more preferably 830-840°C; the moving rate of the continuous annealing is preferably 6-18 m / min, more preferably 8-16 m / min, and further preferably 10-14 m / min. The present invention can control the grain size in the alloy to 0.01-0.015*100 times by controlling the parameters of the continuous annealing, and refine the grains to reduce the risk of alloy cracking.

[0050] After obtaining the annealed alloy, the present invention sequentially performs finished product rolling and stress relief annealing on the annealed alloy to obtain the corrosion-resistant copper-nickel-iron alloy.

[0051] In the present invention, the total processing rate of the finished product rolling is preferably 15-40%, more preferably 20-35%, and further preferably 25-30%; the number of passes of the finished product rolling is preferably 2-4. The present invention can obtain a product of desired thickness by controlling the parameters of the finished product rolling.

[0052] After the rolling of the finished product is completed, the invention preferably unwinds the rolled product. The invention has no particular limitation on the specific operation of unwinding the product, and the operation well known to those skilled in the art can be adopted.

[0053] In the present invention, the temperature of the stress relief annealing is preferably 380-450°C, more preferably 400-420°C; the holding time of the stress relief annealing is preferably 6-10h, more preferably 8h. The present invention can eliminate the residual internal stress inside the alloy through low temperature continuous annealing, and further improve the performance of the alloy.

[0054] After the stress relief annealing is completed, the present invention preferably performs pickling and straightening on the product of the stress relief annealing to obtain a corrosion-resistant copper-nickel-iron alloy. The present invention has no special limitation on the specific operations of pickling and straightening, and the pickling and straightening operations well known to those skilled in the art can be used.

[0055] The preparation method provided by the present invention can reduce the number of processes and reduce costs through large rolling deformation, and can reduce the risk of product cracking by controlling the grain size in each annealing process; the preparation process is simple, the parameters are easy to control, and it is easy to promote on a large scale in industry.

[0056] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0057] Example 1

[0058] A corrosion resistant copper-nickel-iron alloy, consisting of the following chemical components by mass percentage: Ni: 10.1%, Fe: 1.97%, Mn: 0.52%, Ce: 0.04%, Nb: 0.02% and the balance of copper;

[0059] The preparation method of the corrosion-resistant copper-nickel-iron alloy consists of the following steps:

[0060] (1) mixing alloy raw materials, sequentially smelting and horizontally continuously casting, and then milling to obtain alloy ingots; the temperature of the horizontal continuous casting is 1200° C., and the moving speed of the horizontal continuous casting is 120 mm / min;

[0061] (2) performing preliminary rolling on the alloy ingot obtained in step (1) to obtain a preliminary rolled alloy; the total processing rate of the preliminary rolling is 90%, and the number of preliminary rolling passes is 10;

[0062] (3) subjecting the initially rolled alloy obtained in step (2) to coil annealing and pre-finished product rolling in sequence to obtain a rolled alloy; the holding temperature of the coil annealing is 760° C., the holding time of the coil annealing is 12 h, and after the coil annealing is completed, the grain size of the alloy is controlled to be 0.035 to 0.05*100 times; the total processing rate of the pre-finished product rolling is 62%, and the number of passes of the pre-finished product rolling is 4;

[0063] (4) continuously annealing the rolled alloy obtained in step (3) to obtain an annealed alloy; the continuous annealing temperature is 850° C., the continuous annealing moving rate is 12 m / min, and the grain size of the annealed alloy is controlled to be 0.01 to 0.015*100 times;

[0064] (5) The annealed alloy obtained in step (4) is subjected to finished product rolling, unwinding and stress relief annealing in sequence, and finally pickled and stretched and bent to obtain a corrosion-resistant copper-nickel-iron alloy; the total processing rate of the finished product rolling is 25%, and the number of finished product rolling passes is 2 times; the temperature of the stress relief annealing is 450° C., and the holding time of the stress relief annealing is 8 hours.

[0065] Example 2

[0066] A corrosion resistant copper-nickel-iron alloy, consisting of the following chemical components by mass percentage: Ni: 9.2%, Fe: 1.46%, Mn: 0.93%, Ce: 0.04%, Nb: 0.02% and the balance of copper;

[0067] The preparation method of the corrosion-resistant copper-nickel-iron alloy consists of the following steps:

[0068] (1) mixing alloy raw materials, sequentially smelting and horizontally continuously casting, and then milling to obtain an alloy ingot; the temperature of the horizontal continuous casting is 1190° C., and the moving speed of the horizontal continuous casting is 130 mm / min;

[0069] (2) performing preliminary rolling on the alloy ingot obtained in step (1) to obtain a preliminary rolled alloy; the total processing rate of the preliminary rolling is 80%, and the number of preliminary rolling passes is 10;

[0070] (3) subjecting the initially rolled alloy obtained in step (2) to coil annealing and pre-finished product rolling in sequence to obtain a rolled alloy; the holding temperature of the coil annealing is 740° C., the holding time of the coil annealing is 14 h, and after the coil annealing is completed, the grain size of the alloy is controlled to be 0.035 to 0.05*100 times; the total processing rate of the pre-finished product rolling is 64%, and the number of passes of the pre-finished product rolling is 10 times;

[0071] (4) continuously annealing the rolled alloy obtained in step (3) to obtain an annealed alloy; the continuous annealing temperature is 850° C., the continuous annealing moving rate is 12 m / min, and the grain size of the annealed alloy is controlled to be 0.01 to 0.015*100 times;

[0072] (5) The annealed alloy obtained in the step (4) is subjected to finished product rolling, unwinding and stress relief annealing in sequence, and finally pickled and stretched and bent to obtain a corrosion-resistant copper-nickel-iron alloy; the total processing rate of the finished product rolling is 40%, and the number of finished product rolling passes is 4 times; the temperature of the stress relief annealing is 380° C., and the holding time of the stress relief annealing is 8 hours.

[0073] Example 3

[0074] A corrosion resistant copper-nickel-iron alloy, consisting of the following chemical components by mass percentage: Ni: 10.8%, Fe: 1.13%, Mn: 0.22%, Ce: 0.04%, Nb: 0.02% and the balance of copper;

[0075] The preparation method of the corrosion-resistant copper-nickel-iron alloy consists of the following steps:

[0076] (1) mixing alloy raw materials, sequentially performing smelting and horizontal continuous casting, and then performing surface milling to obtain an alloy ingot; the temperature of the horizontal continuous casting is 1210° C., and the moving speed of the horizontal continuous casting is 130 mm / min;

[0077] (2) performing preliminary rolling on the alloy ingot obtained in step (1) to obtain a preliminary rolled alloy; the total processing rate of the preliminary rolling is 86%, and the number of preliminary rolling passes is 10;

[0078] (3) the initially rolled alloy obtained in step (2) is subjected to coil annealing and pre-finished product rolling in sequence to obtain a rolled alloy; the holding temperature of the coil annealing is 720° C., the holding time of the coil annealing is 16 h, and after the coil annealing is completed, the grain size of the alloy is controlled to be 0.035 to 0.05*100 times; the total processing rate of the pre-finished product rolling is 52%, and the number of passes of the pre-finished product rolling is 4 times;

[0079] (4) continuously annealing the rolled alloy obtained in step (3) to obtain an annealed alloy; the continuous annealing temperature is 850° C., the continuous annealing moving rate is 12 m / min, and the grain size of the annealed alloy is controlled to be 0.01 to 0.015*100 times;

[0080] (5) The annealed alloy obtained in step (4) is subjected to finished product rolling, unwinding and stress relief annealing in sequence, and finally pickled and stretched and bent to obtain a corrosion-resistant copper-nickel-iron alloy; the total processing rate of the finished product rolling is 20%, and the number of finished product rolling passes is 2 times; the temperature of the stress relief annealing is 450° C., and the holding time of the stress relief annealing is 8 hours.

[0081] Comparative Example 1

[0082] A copper alloy, comprising, by mass percentage, the following chemical composition: Ni: 0.3%, Sn: 1.9%, P: 0.05% and the balance of copper;

[0083] The preparation method of the copper alloy is the same as that of Example 1.

[0084] Comparative Example 2

[0085] The temperature of horizontal continuous casting in step (1) is 1280°C, and other conditions are the same as those in Example 1.

[0086] Comparative Example 3

[0087] The holding temperature for annealing the ring material in step (3) is 800° C., and other conditions are the same as those in Example 1.

[0088] Comparative Example 4

[0089] Step (4) was omitted in the preparation method, and other conditions were the same as those in Example 1.

[0090] The properties of the alloys prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were tested, and the results are shown in Table 1:

[0091] Table 1 Properties of alloys prepared in Examples 1 to 3 and Comparative Examples 1 to 4

[0092] Tensile strength / MPa Yield strength / MPa Hardness / HV <![CDATA[Elongation rate / A 50 / %]]> Example 1 430 382 138 10.0 Example 2 462 434 151 8.0 Example 3 400 334 130 12.0 Comparative Example 1 358 315 102 11.3 Comparative Example 2 - - - - Comparative Example 3 386 329 123 10.6 Comparative Example 4 371 314 118 10.9

[0093] Among them, the test methods for tensile strength and yield strength are: GB / T 34505-2017 "Room Temperature Tensile Test Method for Copper and Copper Alloy Materials";

[0094] The test method for elongation is: GB / T 34505-2017 "Room Temperature Tensile Test Method for Copper and Copper Alloy Materials";

[0095] The test method for hardness is: GB / T 4340.1-2009 "Vickers hardness method for metal materials".

[0096] It can be seen from Table 1 that the corrosion-resistant copper-nickel-iron alloy provided by the present invention has high tensile strength and yield strength, high hardness and good elongation performance, wherein: when comparative example 1 selects copper alloys of other materials, the performance of the alloy is significantly reduced, indicating that the present invention significantly improves the performance of the copper alloy by optimizing the alloy composition; there is no performance test result for comparative example 2, because the temperature of horizontal continuous casting is too high, and the alloy cannot be cooled quickly during the casting process, resulting in the alloy breaking and being scrapped; the performance of comparative example 3 is reduced, indicating that the annealing temperature of the ring material is too high, which will cause the grains inside the alloy to be large and affect its mechanical properties; the performance of comparative example 4 is reduced, indicating that if continuous annealing is not performed after the pre-finished product is rolled, it will cause large internal stress, which will greatly affect the performance of the alloy during subsequent processing.

[0097] The corrosion resistance of the anti-corrosion copper-nickel-iron alloy provided in Example 1 was tested by an 8-hour salt spray test. Figure 1 As shown. Figure 1 It can be seen that after the 8h salt spray test, the corrosion-resistant copper-nickel-iron alloy provided by the present invention has no obvious corrosion on the surface, indicating that it has excellent corrosion resistance.

[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A corrosion-resistant copper-nickel-iron alloy, comprising the following chemical components by mass percentage: Ni: 4.0-11.0%, Fe: 1.0-2.0%, Mn: 0.2-1.0%, Ce: 0.02-0.05%, Nb: 0.005-0.025% and the balance of copper.

2. The corrosion-resistant copper-nickel-iron alloy according to claim 1, characterized in that: Calculated by mass percentage, it includes the following chemical components: Ni: 7.0-11.0%, Fe: 1.1-1.9%, Mn: 0.2-0.9%, Ce: 0.03-0.05%, Nb: 0.01-0.02% and the balance of copper.

3. The corrosion-resistant copper-nickel-iron alloy according to claim 2, characterized in that: Calculated by mass percentage, the alloy comprises the following chemical components: Ni: 9.0-11.0%, Fe: 1.2-1.9%, Mn: 0.22-0.85%, Ce: 0.04%, Nb: 0.02% and the balance of copper.

4. The method for preparing the corrosion-resistant copper-nickel-iron alloy according to any one of claims 1 to 3, comprising the following steps: (1) mixing alloy raw materials, sequentially melting and horizontally continuously casting to obtain alloy ingots; (2) performing initial rolling on the alloy ingot obtained in step (1) to obtain an initial rolled alloy; (3) subjecting the initially rolled alloy obtained in step (2) to coil annealing and pre-finished product rolling in sequence to obtain a rolled alloy; (4) continuously annealing the rolled alloy obtained in step (3) to obtain an annealed alloy; (5) The annealed alloy obtained in step (4) is subjected to finished product rolling and stress relief annealing in sequence to obtain a corrosion-resistant copper-nickel-iron alloy.

5. The preparation method according to claim 4, characterized in that: In the step (1), the temperature of the horizontal continuous casting is 1190-1210° C., and the moving speed of the horizontal continuous casting is 110-130 mm / min.

6. The preparation method according to claim 4, characterized in that: In the step (3), the heat preservation temperature of the ring material annealing is 720-760° C., and the heat preservation time of the ring material annealing is 12-16 hours.

7. The preparation method according to claim 4, characterized in that: In the step (3), the total processing rate of the pre-finished product rolling is 50-70%, and the number of passes of the pre-finished product rolling is 4-10 times.

8. The preparation method according to claim 4, characterized in that: The temperature of the continuous annealing in the step (4) is 820-850° C., and the moving speed of the continuous annealing is 6-18 m / min.

9. The preparation method according to claim 4, characterized in that: The total processing rate of the finished product rolling in the step (5) is 15-40%, and the number of passes of the finished product rolling is 2-4 times.

10. The preparation method according to claim 4, characterized in that: The temperature of the stress relief annealing in the step (5) is 380-450°C.