High-thermal-conductivity cast aluminum alloy

By optimizing the composition and preparation method of aluminum alloy, a high melting point eutectic phase is formed, which solves the problem of difficult to take into account both the thermal conductivity and strength of existing cast aluminum alloys, and achieves aluminium alloy material with high thermal conductivity, high strength and excellent casting performance.

CN119082566APending Publication Date: 2024-12-06TIANMUSHAN LABORATORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411272436.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing cast aluminum alloys are difficult to maintain high strength and excellent die-casting properties while improving thermal conductivity, and the precious metal elements added to commonly used alloys limit their wide application.

Method used

By optimizing the composition of the aluminum alloy, it includes Cu: 2.7% to 7.5%, Ca: 0.5% to 2.5%, Fe: 0.08% to 1.0%, B≤0.08%, and using specific preparation methods and aging treatments, the high-quality production process is formed The Al8Cu4Ca and Al7Cu2Fe eutectic phases at the melting point inhibit the formation of the Al2Cu eutectic phase and improve the thermal conductivity and strength of the alloy.

Benefits of technology

The high thermal conductivity and high strength of aluminum alloy are achieved, while shortening the solidification interval, reducing thermal cracking, improving casting performance, ensuring the stability and wide application of the alloy at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082566A_ABST
    Figure CN119082566A_ABST
Patent Text Reader

Abstract

The invention discloses a high-thermal-conductivity cast aluminum alloy, and belongs to the technical field of high-performance aluminum alloys. The high-thermal-conductivity cast aluminum alloy comprises the following components in percentage by mass: 2.7%-7.5% of Cu, 0.5%-2.5% of Ca, 0.08%-1.0% of Fe, less than or equal to 0.08% of B, less than or equal to 0.05% of P, less than or equal to 0.05% of S, less than or equal And the balance of Al and inevitable impurities. Through reasonable compatibility of Cu and Ca elements, addition of Fe and B elements and the preparation method of collaborative smelting, casting or die-casting and aging treatment, formation of an Al2Cu eutectic phase is inhibited, an Al8Cu4Ca eutectic structure and an Al7Cu2Fe eutectic structure with higher melting points are formed, and an (Al) + Al8Cu4Ca eutectic reaction and an (Al) + Al7Cu2Fe eutectic reaction are carried out on the alloy at high temperature, so that the solidification interval of the alloy is shortened; and the hot crack of the alloy is reduced, so that the alloy has excellent casting performance. Meanwhile, an Al8Cu4Ca phase and an Al7Cu2Fe phase which are formed at a high eutectic temperature reduce the content of the Cu element in an aluminum matrix, and the heat-conducting property of the alloy is improved. Therefore, the high-thermal-conductivity cast aluminum alloy has wide application prospects in the fields of electronic communication, new energy automobiles and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-performance aluminum alloys, and in particular relates to a high thermal conductivity casting aluminum alloy. Background Art

[0002] Cast aluminum alloys have been widely used in industries such as automobiles, aerospace, and electronic communications. In order to obtain excellent strength and casting properties, a large amount of alloying elements such as Si, Cu, and Mg are usually added to cast aluminum alloys. The addition of these alloying elements will cause the thermal conductivity and electrical conductivity of the alloy to decrease rapidly. With the rapid development of 5G communications, 3C electronics, and new energy vehicles, the demand for aluminum alloys with high thermal conductivity and excellent casting properties is growing, and the commonly used cast aluminum alloys can no longer meet the use requirements. In order to improve the thermal conductivity of die-cast aluminum alloys, researchers are committed to developing new high thermal conductivity die-cast aluminum alloys. Patent CN115976372B discloses a high thermal conductivity and high strength die-cast aluminum alloy material. The invention adds Ag to the aluminum alloy to ensure the strength of the aluminum alloy while making the thermal conductivity of the aluminum alloy reach 180W / (mK). However, Ag is an expensive element, which limits the wide application of alloys. Patent CN114672697B discloses a high thermal conductivity die-cast aluminum alloy, which includes the following components by mass percentage: Ni: 1.5-2.5%, Fe: 0.5-1.5%, Mg: 0.5-1.0%, Zn: 0.9-1.8%, B: 0.1-0.3%, other inevitable impurities: <0.3%, and the balance is Al. The thermal conductivity of the die-cast aluminum alloy is close to 210W / (m·K), but the tensile strength is lower than 210MPa.

[0003] Al-Cu cast aluminum alloys have the characteristics of high strength and heat treatment strengthening, but because Al-Cu alloys have a large tendency to hot cracking and are easy to form loose, they are generally not suitable for die casting. Patent application CN116987937A discloses an Al-Cu-Mn-Ca alloy and a preparation method thereof. The raw materials of the alloy are calculated by mass percentage, including: Cu: 4% to 5%, Mn: 0.5% to 1%, Ca: 0.5% to 1%, Ti: 0.1% to 0.3%, and the balance is Al; the total amount of impurities such as Fe, Si, and Mg is less than 0.2%. The invention forms an (Al) + Al4Ca eutectic structure between grains through the preparation method of extrusion casting, which can effectively reduce the hot cracking tendency of the alloy and increase the casting performance of the Al-Cu-Mn alloy. However, since the Cu element mainly exists in the form of solid solution and Al2Cu in the matrix, the thermal conductivity of the alloy will decrease. In addition, the Mn element will also significantly reduce the thermal conductivity of the aluminum alloy. Therefore, the research and development of Al-Cu aluminum alloys with high thermal conductivity, high strength and excellent die-casting properties is of great significance to expanding the application of aluminum alloys. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a high thermal conductivity cast aluminum alloy.

[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a high thermal conductivity casting aluminum alloy, by adjusting the component content and optimizing the preparation method, the thermal conductivity, strength and die-casting performance of the aluminum alloy are improved at the same time;

[0006] The high thermal conductivity cast aluminum alloy comprises the following elements in percentage by weight: Cu: 2.7% to 7.5wt.%, Ca: 0.5% to 2.5wt.%, Fe: 0.08% to 1.0wt.%, B≤0.08%; the remainder is Al and unavoidable impurities;

[0007] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0008] (1) preheating a crucible and placing an Al ingot therein, heating the crucible to melt the Al ingot, and then heating the crucible to 720-750° C., adding Al-Cu, Al-Ca, Al-Fe, and Al-B master alloys in batches, stirring the mixture thoroughly after melting, and skimming off the slag to obtain an alloy melt;

[0009] (2) introducing Ar gas to refine the alloy melt;

[0010] (3) After the refining is completed, the alloy is allowed to stand for a period of time to remove the scum on the surface, and then cast or die-cast to obtain a cast alloy;

[0011] (4) The cast alloy is subjected to aging treatment to obtain a high thermal conductivity cast aluminum alloy.

[0012] The present invention controls the mass ratio of Cu and Ca in the high thermal conductivity cast aluminum alloy within the range of 4.0≤Cu / Ca≤8.5, thereby ensuring that the alloy fully utilizes the strengthening effect of the network Al8Cu4Ca eutectic phase under the premise of having excellent casting performance, so that the alloy obtains good strength and plasticity. If the mass ratio of Cu and Ca is not within the range of 4.0≤Cu / Ca≤8.5, the Al8Cu4Ca eutectic phase and the Al7Cu2Fe eutectic phase cannot be generated, resulting in a significant decrease in the strength and plasticity and thermal conductivity of the alloy material.

[0013] In the present invention, the Fe element is added to reduce the sticking of the die during the die casting process, but too high a Fe content will form a needle-shaped iron-rich phase, which will significantly reduce the plasticity of the alloy. The presence of the Ca element can have a degenerative effect on the iron-rich phase, reduce the damage to the plasticity of the needle-shaped iron-rich phase, and make the cast aluminum alloy have a higher tolerance for the Fe element. The B element is added in the form of an Al-B master alloy to refine the grain size of the alloy.

[0014] As a preferred embodiment of the present invention, the refining treatment is carried out at a temperature of 720°C and for 30 minutes.

[0015] As a preferred embodiment of the present invention, the aging treatment temperature is 150-250°C and the time is 1-8h, which can reduce the content of Cu element in the aluminum matrix, thereby further improving the thermal conductivity of the alloy, and at the same time forming Al8Cu4Ca precipitation phase in the matrix, inhibiting Al2Cu phase, improving the strength of the alloy while still maintaining high plasticity. Through comparative studies, it is found that too high aging temperature is not conducive to improving thermal conductivity and will reduce the plasticity of the alloy.

[0016] Compared with the prior art, the invention has the following beneficial effects: the invention suppresses the formation of Al2Cu eutectic phase through the rational combination of Cu and Ca elements, the addition of Fe and B elements and the optimization of the synergistic preparation method, forms Al8Cu4Ca eutectic structure and Al7Cu2Fe eutectic structure with higher melting point, and makes the alloy undergo (Al)+Al8Cu4Ca eutectic reaction and (Al)+Al7Cu2Fe eutectic reaction at high temperature, thereby shortening the solidification range of the alloy, reducing the thermal cracking of the alloy, and making the alloy have excellent casting performance. At the same time, the Al8Cu4Ca phase and Al7Cu2Fe phase formed at high eutectic temperature reduce the content of Cu element in the aluminum matrix and improve the thermal conductivity of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 XRD spectra of the die-cast aluminum alloys prepared in Example 1 and Example 4: (a) is the die-cast aluminum alloy prepared in Example 1; (b) is the die-cast aluminum alloy prepared in Example 4.

[0018] Figure 2 SEM images of the die-cast aluminum alloys prepared in Example 1 and Example 4: (a) is the die-cast aluminum alloy prepared in Example 1; (b) is the die-cast aluminum alloy prepared in Example 4. DETAILED DESCRIPTION

[0019] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0020] Example 1

[0021] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 4.2%, Ca: 0.56%, Fe: 0.15%, and the balance is Al and inevitable impurities.

[0022] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0023] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 720° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0024] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0025] (3) After refining, let it stand for 1 hour to remove the surface scum.

[0026] (4) Clean the iron mold and preheat it to 200℃.

[0027] (5) Pouring.

[0028] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0029] (7) The gravity cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 200° C. and the time is 5 h to obtain a gravity cast aluminum alloy.

[0030] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0031] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 720° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0032] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0033] (3) After refining, cool to 680℃ and let stand for 1 hour to remove surface scum.

[0034] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 230°C, first-stage fast pressing speed 0.2m / s, second-stage fast pressing speed 3m / s, and boost pressure 70MPa.

[0035] (5) Fill the mold cavity and maintain pressure for 4 seconds.

[0036] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0037] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 200° C. and the time is 5 h to obtain a die-cast aluminum alloy.

[0038] Example 2

[0039] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 6.1%, Ca: 0.76%, Fe: 0.35%, B: 0.02%, and the balance is Al and inevitable impurities.

[0040] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0041] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 750° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0042] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0043] (3) After refining, let it stand for 1 hour to remove the surface scum.

[0044] (4) Clean the iron mold and preheat it to 200℃.

[0045] (5) Pouring.

[0046] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0047] (7) The gravity cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 250° C. and the time is 1 h to obtain a gravity cast aluminum alloy.

[0048] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0049] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 750° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0050] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0051] (3) After refining, cool to 680℃ and let stand for 1 hour to remove surface scum.

[0052] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 250°C, first-stage fast pressing speed 0.16m / s, second-stage fast pressing speed 3.5m / s, and boost pressure 80MPa.

[0053] (5) Fill the mold cavity and maintain pressure for 5 seconds.

[0054] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0055] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 250° C. and the time is 1 h to obtain a die-cast aluminum alloy.

[0056] Example 3

[0057] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 6.72%, Ca: 1.23%, Fe: 0.78%, B: 0.06%, and the balance is Al and inevitable impurities.

[0058] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0059] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 740° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0060] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0061] (3) After refining, let it stand for 1 hour to remove the surface scum.

[0062] (4) Clean the iron mold and preheat it to 200℃.

[0063] (5) Pouring.

[0064] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0065] (7) The gravity cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 150° C. and the time is 8 h to obtain a gravity cast aluminum alloy.

[0066] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0067] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 740° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0068] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0069] (3) After refining, cool to 700℃ and let stand for 1 hour to remove surface scum.

[0070] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 250°C, first-stage fast pressing speed 0.12m / s, second-stage fast pressing speed 3.5m / s, and boost pressure 80MPa.

[0071] (5) Fill the mold cavity and maintain pressure for 4 seconds.

[0072] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0073] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 150° C. and the time is 8 h to obtain a die-cast aluminum alloy.

[0074] Example 4

[0075] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 7.13%, Ca: 1.69%, Fe: 0.92%, B: 0.07%, and the balance is Al and inevitable impurities.

[0076] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0077] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 720° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0078] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0079] (3) After refining, let it stand for 1 hour to remove the surface scum.

[0080] (4) Clean the iron mold and preheat it to 200℃.

[0081] (5) Pouring.

[0082] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0083] (7) The gravity cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 200° C. and the time is 5 h to obtain a gravity cast aluminum alloy.

[0084] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0085] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 720° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0086] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0087] (3) After refining, cool to 700℃ and let stand for 1 hour to remove surface scum.

[0088] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 250°C, first-stage fast pressing speed 0.16m / s, second-stage fast pressing speed 3m / s, and boost pressure 80MPa.

[0089] (5) Fill the mold cavity and maintain pressure for 3 seconds.

[0090] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0091] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 200° C. and the time is 5 h to obtain a die-cast aluminum alloy.

[0092] Figure 1 The XRD patterns of the die-cast aluminum alloys of Example 1 and Example 4 are shown in FIG. Figure 1 (a) It can be seen that the phase composition of the die-cast alloy of Example 1 is α-Al and Al8Cu4Ca phase. When the content of Cu and Ca is increased ( Figure 1b), the second phase is still Al8Cu4Ca phase. In addition, due to the high Fe content, Al7Cu2Fe phase is formed in the alloy.

[0093] Figure 2 Figure 1 is a scanning electron microscope image of the die-cast alloys of Example 1 and Example 4. It can be seen that the Al8Cu4Ca phase in the die-cast alloy of Example 1 is distributed in a network form ( Figure 2 a), with the increase of Cu and Fe content, in Example 4, in addition to the network-like Al8Cu4Ca eutectic phase, strip-like Al7Cu2Fe ( Figure 2 b) The formation of Al8Cu4Ca and Al7Cu2Fe phases reduces the content of Cu in the aluminum matrix. Energy spectrum analysis shows that the mass fraction of Cu in the alloy matrix of Example 4 is only 1.1%.

[0094] Comparative Example 1

[0095] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 6.1%, Fe: 0.35%, B: 0.02%, and the balance is Al and inevitable impurities.

[0096] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0097] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 750° C., Al-Cu, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0098] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0099] (3) After refining, cool to 680℃ and let stand for 1 hour to remove surface scum.

[0100] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 250°C, first fast speed 0.2m / s, second fast speed 3.5m / s, and boost pressure 80MPa.

[0101] (5) Fill the mold cavity and maintain pressure.

[0102] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0103] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 250° C. and the time is 1 h to obtain a die-cast aluminum alloy.

[0104] Comparative Example 2

[0105] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 6.1%, Ca: 0.76%, B: 0.02%, and the balance is Al and inevitable impurities.

[0106] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0107] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 750° C., Al-Cu, Al-Ca and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0108] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0109] (3) After refining, cool to 680℃ and let stand for 1 hour to remove surface scum.

[0110] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 250°C, first fast speed 0.2m / s, second fast speed 3.5m / s, and boost pressure 80MPa.

[0111] (5) Fill the mold cavity and maintain pressure.

[0112] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0113] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 250° C. and the time is 1 h to obtain a die-cast aluminum alloy.

[0114] Comparative Example 3

[0115] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 6.1%, Ca: 0.76%, Fe: 1.4%, B: 0.02%, and the balance is Al and inevitable impurities.

[0116] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0117] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 750° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0118] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0119] (3) After refining, cool to 680℃ and let stand for 1 hour to remove surface scum.

[0120] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 250°C, first fast speed 0.2m / s, second fast speed 3.5m / s, and boost pressure 80MPa.

[0121] (5) Fill the mold cavity and maintain pressure.

[0122] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0123] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 250° C. and the time is 1 h to obtain a die-cast aluminum alloy.

[0124] Comparative Example 4

[0125] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 6.1%, Ca: 0.3%, Fe: 0.35%, B: 0.02%, and the balance is Al and inevitable impurities.

[0126] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0127] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 750° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0128] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0129] (3) After refining, cool to 680℃ and let stand for 1 hour to remove surface scum.

[0130] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 250°C, first fast speed 0.2m / s, second fast speed 3.5m / s, and boost pressure 80MPa.

[0131] (5) Fill the mold cavity and maintain pressure.

[0132] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0133] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 250° C. and the time is 1 h to obtain a die-cast aluminum alloy.

[0134] Comparative Example 5

[0135] A high thermal conductivity cast aluminum alloy comprises the following components in percentage by mass: Cu: 1.5%, Ca: 0.76%, Fe: 0.35%, B: 0.02%, and the balance is Al and inevitable impurities.

[0136] The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps:

[0137] (1) Raw materials are quantitatively prepared according to the mass percentage, wherein the raw materials include Al ingot, Al-Cu, Al-Ca, Al-Fe and Al-B master alloy; the crucible is preheated and loaded with the Al ingot, the temperature is increased to melt the Al ingot, the temperature is increased to 750° C., Al-Cu, Al-Ca, Al-Fe and Al-B master alloy are added in batches, the mixture is fully stirred after melting, and slag is removed to obtain an alloy melt.

[0138] (2) Ar gas was introduced into the alloy melt and the alloy melt was refined at 720°C for 30 min.

[0139] (3) After refining, cool to 680℃ and let stand for 1 hour to remove surface scum.

[0140] (4) A 450t cold chamber die casting machine was used for die casting. The die casting process parameters were as follows: mold temperature 250°C, first fast speed 0.2m / s, second fast speed 3.5m / s, and boost pressure 80MPa.

[0141] (5) Fill the mold cavity and maintain pressure.

[0142] (6) Open the mold and take out the cast alloy, which is recorded as F.

[0143] (7) The die-cast alloy is subjected to T5 aging treatment to obtain a high thermal conductivity cast aluminum alloy. The temperature of the T5 aging treatment is 250° C. and the time is 1 h to obtain a die-cast aluminum alloy.

[0144] Effect example

[0145] Test samples: aluminum alloys prepared in Examples 1-4 and aluminum alloys prepared in Comparative Examples 1-5.

[0146] Test method: The thermal conductivity of the cast and aged alloys was tested using a laser thermal conductivity meter, and the tensile properties of the alloy were tested using a universal mechanical testing machine. The results are shown in Table 1.

[0147] Table 1

[0148]

[0149] As shown in Table 1, in Examples 1-4, compared with the gravity cast aluminum alloy, the thermal conductivity of the die-cast aluminum alloy is similar to that of the gravity cast aluminum alloy, but the alloy strength is significantly improved. In Examples 1-4, due to the increase in the content of Cu, Ca, and Fe elements, the content of the eutectic phase increases, which makes the thermal conductivity of the alloy basically unchanged while improving the tensile properties of the alloy. The thermal conductivity of all die-cast alloys is greater than 200W / (mK), and the tensile strength is greater than 290MPa.

[0150] Compared with Comparative Examples 1 and 4 and Examples 1-4, Ca has a great influence on the strength, plasticity and thermal conductivity of the alloy. Due to the lack of Ca element, the solidification range of the alloy is relatively wide, thermal cracks exist in the die-casting specimen, and the tensile specimen breaks without obvious plastic deformation, resulting in poor strength and plasticity of the alloy. In addition, due to the lack of Ca, the Cu element content in the matrix is ​​relatively high, resulting in a low thermal conductivity of the die-casting alloy. The amount of Ca added to the alloy is small, an Al2Cu eutectic phase is formed in the die-casting alloy, and the plasticity of the needle-shaped iron-rich phase is damaged, resulting in a decrease in the strength and plasticity of the alloy, and the thermal conductivity of the die-casting alloy is also decreased.

[0151] According to Comparative Examples 2, 3 and Examples 1-4, it can be seen that the lack of Fe element leads to the phenomenon of sticking to the die during the die casting process, which increases the casting defects in the structure and reduces the plasticity of the alloy. In addition, due to the absence of the formation of Al7Cu2Fe phase, the Cu content in the aluminum matrix increases, resulting in a decrease in the thermal conductivity of the die casting alloy. Although the high Fe content in Comparative Example 3 can avoid sticking to the die during the die casting process, the excessive addition of Fe element reduces the plasticity of the alloy and increases the thermal resistance generated by the phase interface, thereby reducing the thermal conductivity. If the Fe element content is too low, the Al7Cu2Fe phase cannot be generated, which will cause die sticking in the die casting and reduce the thermal conductivity of the alloy. Al7Cu2Fe can only be generated when the Fe content is above 0.15%, which has a more obvious effect on reducing the thermal conductivity of the alloy.

[0152] According to Comparative Example 5 and Examples 1-4, the Cu content is low, the casting fluidity of the alloy is poor, resulting in low plasticity of the alloy, and since only a small amount of Al4Ca and Al6Fe second phases exist in the solidified structure, the strength of the die-casting alloy is also reduced.

[0153] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A high thermal conductivity cast aluminum alloy, characterized in that: By adjusting the component content and optimizing the preparation method, the thermal conductivity, strength and die-casting performance of aluminum alloys are improved at the same time; The high thermal conductivity cast aluminum alloy comprises the following elements in percentage by weight: Cu: 2.7% to 7.5wt.%, Ca: 0.5% to 2.5wt.%, Fe: 0.08% to 1.0wt.%, B≤0.08%; the remainder is Al and unavoidable impurities; The method for preparing the high thermal conductivity cast aluminum alloy comprises the following steps: (1) After melting the Al ingot, the temperature is raised to 720-750° C., and Al-Cu, Al-Ca, Al-Fe and Al-B master alloys are added in batches. After melting, the mixture is fully stirred and slag is removed to obtain an alloy melt; (2) introducing Ar gas to refine the alloy melt; (3) After the refining is completed, the alloy is allowed to stand for a period of time to remove the scum on the surface, and then cast or die-cast to obtain a cast alloy; (4) The cast alloy is subjected to aging treatment to obtain a high thermal conductivity cast aluminum alloy.

2. The high thermal conductivity cast aluminum alloy according to claim 1, characterized in that: The mass ratio of Cu to Ca in the high thermal conductivity cast aluminum alloy is 4.0≤Cu / Ca≤8.

5.

3. The high thermal conductivity cast aluminum alloy according to claim 1, characterized in that: The refining treatment was carried out at a temperature of 720° C. and for 30 minutes.

4. The high thermal conductivity cast aluminum alloy according to claim 1, characterized in that: The temperature of the aging treatment is 150-250° C., and the time is 1-8 hours.