Plastic die steel and preparation method thereof

Through the optimization of specific components and forging process, the problem of insufficient hardness and tissue uniformity of plastic mold steel is solved, and high hardness and high precision plastic mold steel preparation is achieved, meeting the high requirements of the home appliance industry.

CN119082612APending Publication Date: 2024-12-06PANGANG GROUP JIANGYOU CHANGCHENG SPECIAL STEEL COMPANY LIMITED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411361453.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The hardness uniformity and tissue uniformity of existing plastic mold steels are insufficient, resulting in poor processing performance and short service life, making it difficult to meet the requirements of the home appliance industry for high precision and high hardness.

Method used

Plastic mold steel with specific components, including C 0.31~0.36%, Si 0.25~0.40%, Mn 0.55~0.80%, Cr 7.50~8.50%, Ni 0.10~0.30%, Mo 0.50~0.70%, V 0.50~0.70% , Al 0.01~0.04%, [N] 0.035~0.045%, and optimized by high-temperature heating, annealing and quenching processes before forging, combining three upsetting and FM forging methods to ensure uniform distribution of alloy elements and spherical distribution of carbides, improving Hardness and tissue uniformity of steel ingots.

Benefits of technology

It realizes the hardness and tissue uniformity of plastic mold steel, improves the comprehensive performance of steel ingots, extends the service life, and meets the requirements of high precision and high hardness in the home appliance industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides plastic die steel which comprises the following components in percentage by mass: 0.31 to 0.36 percent of C, 0.25 to 0.40 percent of Si, 0.55 to 0.80 percent of Mn, 7.50 to 8.50 percent of Cr, 0.10 to 0.30 percent of Ni, 0.50 to 0.70 percent of Mo, 0.50 to 0.70 percent of V, 0.01 to 0.04 percent of Al, 0.035 to 0.045 percent of [N] and the balance of Fe. The invention further provides a preparation method of the plastic die steel. According to the plastic die steel and the preparation method thereof, the high-quality and large-section plastic die steel is prepared by regulating and controlling the components of the plastic die steel and adopting the preparation method of steel ingot forging and a special heat treatment process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mold steel, and in particular to a plastic mold steel and a preparation method thereof. Background Art

[0002] Mold steel is a steel material used to manufacture injection molds, cold stamping molds, hot forging molds, die-casting molds and other molds. Its quality directly affects the quality of pressure processing technology, product precision output and production cost. Plastic mold steel is a new type of mold steel that has been developed. Generally, plastic mold steel is obtained by quenching and tempering 45 and 40Cr after normalizing. Therefore, the mold steel has low hardness, poor wear resistance, high surface roughness value, and the appearance quality of the processed plastic products is poor, and the mold steel has a short service life; while precision plastic mold steel and high hardness plastic mold steel are prepared by alloy tool steels such as CrWMo and Cr12MoV. Not only do they have poor machining performance, but they are also difficult to process complex cavities, and cannot solve the problem of heat treatment deformation.

[0003] Plastic mold steel has also been widely used in home appliance molds, but the hard spots in plastic mold steel can easily lead to tool breakage during the processing process. On the other hand, the home appliance industry has high requirements, and the cost and impact caused by the failure of the mold after use are large, so it is necessary to ensure that the finished product structure and hardness uniformity are extremely high. Summary of the invention

[0004] The technical problem solved by the present invention is to provide a plastic mold steel and a preparation method thereof. The plastic mold steel provided by the present application can ensure the uniformity of structure and hardness.

[0005] In view of this, the present application provides a plastic mold steel, which includes, by mass percentage, C 0.31~0.36%, Si 0.25~0.40%, Mn 0.55~0.80%, Cr 7.50~8.50%, Ni 0.10~0.30%, Mo 0.50~0.70%, V 0.50~0.70%, Al 0.01~0.04%, [N] 0.035~0.045%, and the balance is Fe.

[0006] Preferably, the plastic mold steel has P≤0.20%, S≤0.005%, and [O]≤0.0020%.

[0007] Preferably, the plastic mold steel comprises: C 0.33~0.35%, Si 0.31~0.39%, Mn 0.62~0.75%, Cr7.96~8.40%, Ni 0.19~0.28%, Mo 0.62~0.68%, V 0.59~0.68%, Al 0.02~0.03%, [N] 0.038~0.042%, P≤0.15%, S≤0.002%, [O]≤0.0015%, and the balance is Fe.

[0008] The present application also provides a method for preparing the plastic mold steel, comprising the following steps:

[0009] S1) heating the steel ingot to 550-650°C, heating to 800-900°C after the first heat preservation, heating to 1200-1300°C after the second heat preservation, and then heating for the third time; the composition of the steel ingot is the composition of the plastic mold steel according to any one of claims 1 to 3;

[0010] S2) forging the steel ingot obtained in step S1), and annealing the forged steel ingot;

[0011] S3) the steel ingot obtained in step S2) is heated to 800-900°C after the first heat preservation at 200-300°C, heated to 1000-1100°C after the second heat preservation, and quenched after the third heat preservation;

[0012] S4) The quenched steel ingot is tempered.

[0013] Preferably, the start forging temperature of the forging is ≥1050°C, and the final forging temperature is ≥850°C; the forging adopts a forging method combining three upsetting and FM method, and the FM method forging is started after the three upsetting is upset to ≤H0 / 2; H0 is the initial height of the ingot.

[0014] Preferably, the annealing is specifically:

[0015] The forged steel ingot is heated from 400~500℃ to 850~900℃ at a rate of 30~50℃ / h, kept at this temperature for 14~17h, then cooled to 720~750℃ at a rate of 10~30℃ / h, kept at this temperature for 16~19h, then cooled to ≤350℃ and taken out of the furnace.

[0016] Preferably, in step S3), the quenching cooling method is specifically:

[0017] The steel ingot is quenched and cooled in the quenching liquid to a maximum temperature of 300~350℃ in the center of the large surface, and then air-cooled to 80~100℃.

[0018] Preferably, the tempering treatment is specifically:

[0019] The quenched steel ingot is heated to 200-300°C, kept at this temperature for 27-36 hours and then air-cooled.

[0020] Preferably, in step S1), the first insulation time is 5~7h, the heating rate from 550~650℃ to 800~900℃ is 30~50℃ / h, the second insulation time is 6~8h, the heating rate from 800~900℃ to 1200~1300℃ is 70~100℃, and the third insulation time is 20~25h.

[0021] Preferably, in step S3), the first insulation time is 3~6h, the heating rate from 200~300℃ to 800~900℃ is 10~40℃ / h, the second insulation time is 4~6h, the heating rate from 800~900℃ to 1000~1100℃ is 50~80℃ / h, and the third insulation time is 0.015D+2~3h, where D is the thickness of the forged ingot.

[0022] The present application provides a method for preparing plastic mold steel, which comprises the following steps: firstly, heating a steel ingot with a specific heating system, then forging the steel ingot, annealing the forged steel ingot, quenching the steel ingot with a specific quenching system, and finally tempering the steel ingot to obtain the plastic mold steel; the present application adopts a specific heating system before forging to homogenize the steel ingot at high temperature and for a long time, thereby improving segregation and improving the uniform distribution of alloy elements in the steel ingot; the annealing after forging makes the carbides in the steel ingot structure spherical in shape, so as to prepare the structure for subsequent heat treatment; during the quenching process, the specific heating system makes the carbides dissolve into the matrix as much as possible, while ensuring that the grains and martensite laths do not grow out of control; the cooling method makes the matrix uniformly transform into martensite, thereby finally ensuring the hardness and uniform structure of the plastic mold steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a curve diagram of heating before forging in the preparation process of the plastic mold steel of the present invention;

[0024] Figure 2 It is a curve diagram of the annealing process in the preparation process of the plastic mold steel of the present invention;

[0025] Figure 3 It is a curve diagram of the quenching process in the preparation process of the plastic mold steel of the present invention;

[0026] Figure 4 It is a curve diagram of the tempering process in the preparation process of the plastic mold steel of the present invention;

[0027] Figure 5 This is a curve diagram of heating before forging in the preparation process of plastic mold steel in Example 1 of the present invention;

[0028] Figure 6 This is a curve diagram of the annealing process in the preparation process of the plastic mold steel in Example 1 of the present invention;

[0029] Figure 7 This is a curve diagram of the quenching process in the preparation process of the plastic mold steel in Example 1 of the present invention;

[0030] Figure 8 It is a curve diagram of the tempering process in the preparation process of the plastic mold steel in Example 1 of the present invention;

[0031] Fig. 9 This is a metallographic photograph of the plastic mold steel prepared in Example 1 of the present invention;

[0032] Fig.10 This is a metallographic photograph of the plastic mold steel prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0033] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0034] In view of the performance requirements for uniform hardness of plastic mold steel in the prior art, the present invention provides a plastic mold steel and a preparation method thereof, which adopts a specific element ratio and optimizes the pre-forging heating system and the quenching process heating system during the preparation process to achieve uniformity of the structure and hardness of the plastic mold steel; specifically, the present application first provides a plastic mold steel, which comprises, by mass percentage: C 0.31~0.36%, Si 0.25~0.40%, Mn 0.55~0.80%, Cr 7.50~8.50%, Ni 0.10~0.30%, Mo 0.50~0.70%, V 0.50~0.70%, Al 0.01~0.04%, [N] 0.035~0.045%, and the balance is Fe.

[0035] In the plastic mold steel provided in the present application, the contents of P, S and [O] are further limited, specifically, P≤0.20%, S≤0.005%, [O]≤0.0020%.

[0036] In plastic mold steel, C is an austenite-forming element. Increasing the C content can expand the austenite zone and increase the hardness of the steel after quenching. However, if the C content is too high, the toughness of the steel decreases and it is not good for the corrosion resistance of the steel. Therefore, the C content is limited to 0.31-0.36% to take into account both hardenability and corrosion resistance. Specifically, the C content is 0.33-0.35%. For example, the C content in this application is 0.32% and 0.34%.

[0037] The addition of Si is mainly to improve the oxidation resistance and corrosion resistance of steel, and at the same time can reduce the pitting tendency of steel in a chlorine-containing environment; the Si content is 0.25~0.40%, specifically, the Si content is 0.31~0.39%; for example, the Si content in this application is 0.26%, 0.27%, 0.28%, 0.29%, 0.30%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, and 0.38%. The content of Mn is 0.55-0.80%, specifically, the content of Mn is 0.62-0.75%; for example, the content of Mn in this application is 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.70%, 0.71%, 0.72%, 0.73%, 0.74%, 0.76%, 0.77%, 0.78%, and 0.79%.

[0038] At the same time, the appropriate addition of Cr can ensure the corrosion resistance of the steel, and combine with C to form dispersed carbides to ensure wear resistance; the Cr content is 7.50-8.50%, specifically, the Cr content is 7.96-8.40%; for example, the Cr content of the present application is 7.51%, 7.52%, 7.53%, 7.64%, 7.65%, 7.76%, 7.77%, 7.73%, 7.59%, 7.60%, 7.71%, 7.74%, 7.81%, 7.83%, 7.86%, 7.89%, 7.92%, 7.95%, 7.98%, 7.94%, 8.01%, 8.05%, 8.07%, 8.13%, 8.16%, 8.17%, 8.19%, 8.23%, 8.25%, 8.27%, 8.29%, 8.31%, 8.33%, 8.35%, 8.38%, 8.40%, 8.43%, 8.46%, and 8.49%.

[0039] The appropriate addition of Ni can maintain the high temperature austenite zone, and obtaining the quenched martensite structure can make the steel have good comprehensive properties; the Ni content is 0.10~0.30%, specifically, the Ni content is 0.19~0.28%; for example, the Ni content in this application is 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, and 0.29%.

[0040] In order to ensure the hardenability of steel, ensure its tempering stability and corrosion resistance, Mo can be added in an appropriate amount, and the content of Mo is 0.50-0.70%. Specifically, the content of Mo is 0.62-0.68%. By way of example, the content of Mo in this application is 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.59%, 0.60%, 0.61%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, and 0.69%. The V content is 0.50-0.70%, specifically, the V content is 0.59-0.68%; for example, the V content in this application is 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.60%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, and 0.69%.

[0041] The content of Al is 0.01-0.04%, specifically, the content of Al is 0.02% and 0.03%. The addition of N can make carbides or nitrides more evenly and smoothly distributed, thereby avoiding or reducing the number of large-sized carbides and improving the toughness and corrosion resistance of steel; the content of [N] is 0.035-0.045%, specifically, the content of [N] is 0.038-0.042%; for example, the content of [N] is 0.036%, 0.037%, 0.039%, 0.040%, 0.041%, 0.043% and 0.044%.

[0042] Furthermore, P≤0.15%, S≤0.002%, and [O]≤0.0015%.

[0043] The present application also provides a method for preparing plastic mold steel, comprising the following steps:

[0044] S1) heating the steel ingot to 550-650°C, heating to 800-900°C after the first heat preservation, heating to 1200-1300°C after the second heat preservation, and then heating for the third time; the composition of the steel ingot is the composition of the plastic mold steel described above;

[0045] S2) forging the steel ingot obtained in step S1), and annealing the forged steel ingot;

[0046] S3) the steel ingot obtained in step S2) is heated to 800-900°C after the first heat preservation at 200-300°C, heated to 1000-1100°C after the second heat preservation, and quenched after the third heat preservation;

[0047] S4) The quenched steel ingot is tempered.

[0048] In the process of preparing plastic mold steel, the present application gives priority to preparing steel ingots, firstly adopting the process route of electric arc furnace + LF + VD to smelt electrode rods that meet the composition of plastic mold steel, and then remelting the electrode rods in an electric slag furnace under a protective atmosphere to obtain electric slag ingots. The above smelting method is carried out according to the technical means well known to those skilled in the art, and the present application does not impose any special restrictions on this.

[0049] The present application then forges the steel ingot and heats it before forging. The heating system is as follows: Figure 1 As shown, specifically:

[0050] Heat the heating furnace to ≤450℃, place the steel ingot in the heating furnace and heat it to 550~650℃, keep it warm for 5~7h, then heat it to 830~870℃ at a rate of 30~50℃ / h, keep it warm for 6~8h, then heat it to 1245~1265℃ at a rate of 70~100℃ / h, keep it warm for 20~25h before starting forging.

[0051] More specifically, the heating furnace is heated to ≤450°C, the steel ingot is placed in the heating furnace and heated to 560~620°C, kept warm for 5.5~6.5h, then heated to 840~860°C at a rate of 35~45°C / h, kept warm for 6.5~7.5h, then heated to 1250~1260°C at a rate of 80~90°C / h, and kept warm for 23~25h before starting forging.

[0052] For example, the heating furnace is heated to 450°C, the steel ingot is placed in the heating furnace and heated to 590°C, after keeping warm for 5.5 hours, the temperature is increased to 850°C at a rate of 50°C / h, after keeping warm for 7.5 hours, the temperature is increased to 1255°C at a rate of 100°C / h, and forging is started after keeping warm for 23 hours; or, the heating furnace is heated to 450°C, the steel ingot is placed in the heating furnace and heated to 590°C, after keeping warm for 5.5 hours, the temperature is increased to 850°C at a rate of 50°C / h, after keeping warm for 7.0 hours, the temperature is increased to 1255°C at a rate of 100°C / h, and forging is started after keeping warm for 21 hours.

[0053] The above heating system is homogenized at high temperature and for a long time to improve the structural segregation and enhance the uniform distribution of alloy elements.

[0054] The present application then performs forging, and the forging adopts a forging method combining three upsetting and FM method. After the third upsetting of the three upsetting is ≤H0 / 2, the third elongation is performed and then the FM method forging is started; the H0 is the initial height of the steel ingot; in the forging process, specifically: the first upsetting, the first elongation, the second upsetting, the second elongation, the third upsetting, the third elongation, and the FM method. The start forging temperature of the forging is ≥1050℃, and the final forging temperature is ≥850℃. Specifically, the start forging temperature of the forging is 1050~1200℃, and the final forging temperature is 850~950℃. Specifically, the start temperature of the forging is 1100~1150℃, and the final forging temperature is 870~915℃.

[0055] According to the present invention, the forged steel ingot is then annealed, and the annealing system is as follows: Figure 2 As shown, specifically:

[0056] The forged steel ingot is heated from 400~500℃ to 850~900℃ at a rate of 30~50℃ / h, kept at this temperature for 14~17h, then cooled to 720~750℃ at a rate of 10~30℃ / h, kept at this temperature for 16~19h, then cooled to ≤350℃ and taken out of the furnace.

[0057] More specifically, the forged steel ingot is heated from 420-480°C to 860-880°C at a rate of 33-47°C / h, kept at that temperature for 15.5-16.5h, then cooled to 730-745°C at a rate of 13-28°C / h, kept at that temperature for 17.5-18.5h, then cooled to ≤350°C and taken out of the furnace.

[0058] For example, the forged steel ingot is heated from 450°C to 865°C at a rate of 50°C / h, kept at this temperature for 16.5 hours, then cooled to 735°C at a rate of 30°C / h, kept at this temperature for 18.5 hours, then cooled to 350°C and taken out of the furnace; or, the forged steel ingot is heated from 450°C to 865°C at a rate of 50°C / h, kept at this temperature for 14.5 hours, then cooled to 735°C at a rate of 30°C / h, kept at this temperature for 16.5 hours, then cooled to 350°C and taken out of the furnace.

[0059] The annealing is performed to make the carbides in the ingot structure spherical and to prepare the structure for subsequent heat treatment.

[0060] The present application then performs a quenching process on the forged steel ingot. When the steel ingot is loaded into the furnace for quenching, the steel ingot should be placed sideways to avoid deformation. The quenching process is specifically as follows:

[0061] The steel ingot is heated to 800~900℃ after the first heat preservation at 200~300℃, heated to 1000~1100℃ after the second heat preservation, and quenched after the third heat preservation.

[0062] Specifically, the quenching process is as follows: Figure 3As shown, the steel ingot is kept at 200-300℃ for 3-6h, then heated to 830-870℃ at a rate of 10-40℃ / h, kept for 4-6h, then heated to 1035-1055℃ at a rate of 50-80℃ / h, kept for 0.015D+2-3h, and then quenched, where D is the thickness of the steel ingot after forging;

[0063] More specifically, the steel ingot is kept at 230-280°C for 5 hours, then heated to 840-850°C at a rate of 20-30°C / h, kept for 4-5 hours, then heated to 1040-1050°C at a rate of 60-70°C / h, kept for 0.015D+2h, and then quenched, where D is the thickness of the steel ingot after forging.

[0064] For example, the steel ingot is kept at 230°C for 5 hours, then heated to 850°C at a rate of 40°C / h, then heated to 1045°C at a rate of 80°C / h after keeping for 5 hours, and then quenched after keeping for 0.015D+2h; or, the steel ingot is kept at 230°C for 3 hours, then heated to 850°C at a rate of 40°C / h, then heated to 1045°C at a rate of 80°C / h after keeping for 4 hours, and then quenched after keeping for 0.015D+2h.

[0065] The cooling method of quenching specifically refers to placing the ingot after insulation in a quenching liquid and quenching it to a maximum temperature of 300~350℃ in the center of the large surface, and then air cooling it to 80~100℃ for tempering; more specifically, the quenching is placing the ingot after insulation in a quenching liquid and quenching it to a maximum temperature of 320~340℃ in the center of the large surface, and then air cooling it to 85~95℃ for tempering.

[0066] The heating in the above quenching process allows the carbides to dissolve into the matrix as much as possible, while ensuring that the grains and martensite laths do not grow out of control; cooling allows the matrix to be evenly transformed into martensite, ensuring the hardness and uniformity of the material.

[0067] The present invention finally performs tempering treatment on the quenched steel ingot. The process system of the tempering treatment is as follows: Figure 4 As shown, specifically:

[0068] The quenched steel ingot is heated to 200-300°C, kept at this temperature for 27-36 hours and then air-cooled.

[0069] More specifically, the quenched steel ingot is heated to 220-280°C for 5-6 hours, kept at this temperature for 32-35 hours, and then air-cooled;

[0070] Furthermore, the quenched steel ingot was heated to 240-270°C within 6 h, kept at this temperature for 33-34 h, and then air-cooled.

[0071] The above-mentioned tempering treatment is to reduce quenching stress, ensure corresponding organizational transformation, and improve the toughness and plasticity of plastic mold steel.

[0072] The present application provides a plastic mold steel and a preparation method thereof. The present application prepares high-quality, large-section plastic mold steel by regulating the composition of the plastic mold steel and adopting a preparation method of "steel ingot forging + special heat treatment process".

[0073] In order to further understand the present invention, the preparation method of the plastic mold steel provided by the present invention is described in detail below in conjunction with embodiments, and the protection scope of the present invention is not limited by the following embodiments.

[0074] Example 1

[0075] 1. Steelmaking

[0076] The φ570mm electrode rod was smelted by the arc furnace + LF + VD process route, and the φ570mm electrode rod was remelted by the protective atmosphere electroslag furnace to obtain an electroslag ingot with a diameter of φ770mm and a length of 1.9-2.0m. The composition of the electroslag ingot is shown in Table 1, and the remainder is Fe;

[0077] Table 1 Composition data of electroslag ingot in this embodiment (mass percentage)

[0078]

[0079] 2. Forging

[0080] The heating furnace is heated to 450℃, the electroslag ingot is placed in the heating furnace and heated to 590℃ and kept warm for 5.5h, then heated to 850℃ at a rate of 50℃ / h, kept warm for 7.5h, then heated to 1255℃ at a rate of 100℃ / h, kept warm for 24.5h and then started forging. The stage curve of the heating stage is shown in Figure 5 As shown; the starting forging temperature is 1150℃, the forging adopts the forging method combining three times upsetting and drawing + FM method (after three times of upsetting and three times of drawing, the third upsetting to H0 / 2 is followed by the third drawing, and then the FM method is used to draw to the target size), the final forging temperature is 915℃, that is, the steel ingot is taken out of the furnace, and the steel ingot with a width of 710mm and a thickness of 410mm is obtained;

[0081] (3) Post-forging cooling and annealing process:

[0082] The forged ingot is hot loaded into the annealing furnace for annealing. The finished product annealing process is as follows Figure 6 As shown, specifically: the forged steel ingot is cooled to 450°C, heated to 865°C at a rate of 50°C / h, kept at this temperature for 16.5h, cooled to 735°C at a rate of 30°C / h, kept at this temperature for 18.5h, cooled to 350°C and taken out of the furnace;

[0083] 3. Heat treatment process

[0084] (1) Quenching process:

[0085] The forged steel ingot is charged into the furnace for quenching process, such as Figure 7 Specifically, the steel ingot is kept at 230℃ for 5h, heated to 850℃ at a rate of 40℃ / h, kept for 5h and heated to 1045℃ at a rate of 80℃ / h, kept for 8.2h and then placed in quenching liquid for quenching, cooled to a maximum temperature of 326℃ at the center of the large surface, air-cooled to 86℃ and then loaded into the furnace for tempering; when loading the furnace, the steel ingot should be placed on its side;

[0086] (2) Tempering process:

[0087] After quenching, press Figure 8 The curve shown is immediately tempered, specifically: the quenched steel ingot is heated to 250°C in 6 hours, kept at this temperature for 33 hours and then air-cooled to obtain plastic mold steel;

[0088] 4. Hardness uniformity

[0089] The plastic mold steel prepared above was subjected to hardness testing. The hardness test was performed using a portable Leeb hardness tester to test Rockwell hardness. The testing point was located on the diagonal of the end face of the plastic mold steel. A total of 9 points were tested, including the corner, 1 / 4 of the diagonal, and the center. The hardness testing surface required sanding + polishing. The grinding and polishing depth of the black leather surface was >4mm, and the sawn surface was >1mm. The results showed that the cross-sectional hardness range of the plastic mold steel was 42~44HRC.

[0090] 5. The performance is shown in Table 2;

[0091] Table 2 Performance data of plastic mold steel prepared in this example

[0092]

[0093] 6. Tissue uniformity

[0094] The metallographic photograph of the core of the plastic mold steel prepared in this embodiment is as follows: Fig. 9 As shown by Fig. 9 It can be seen that the core structure of the plastic mold steel prepared in this embodiment has good uniformity.

[0095] Example 2

[0096] 1. Steelmaking

[0097] The φ510mm electrode rod was smelted by the arc furnace + LF + VD process route, and the φ510mm electrode rod was remelted in a protective atmosphere electroslag furnace to obtain an electroslag ingot with a diameter of 680mm and a length of 1.6~1.7m. The composition of the electroslag ingot is shown in Table 3, and the remainder is Fe;

[0098] Table 3 Composition data of electroslag ingot in this embodiment (mass percentage)

[0099]

[0100] 2. Forging

[0101] The heating furnace is heated to 450°C, the electroslag ingot is placed in the heating furnace and heated to 590°C for 5.5 hours, then heated to 850°C at a rate of 50°C / h, and kept for 7.0 hours, then heated to 1255°C at a rate of 100°C / h, and kept for 21 hours before forging; the forging temperature is 1150°C, and the forging adopts a forging method combining three times of upsetting and drawing + FM method (after three times of upsetting and three times of drawing, the third upsetting to H0 / 2 is performed and then the third drawing is performed, and then the FM method is used to draw to the target size), the final forging temperature is 907°C, that is, the steel ingot is taken out of the furnace, and a steel ingot with a width of 710 mm and a thickness of 290 mm is obtained;

[0102] (3) Post-forging cooling and annealing process:

[0103] The forged steel ingot is hot loaded into the annealing furnace for annealing, specifically: the forged steel ingot is cooled to 450°C, heated to 865°C at a rate of 50°C / h, kept at this temperature for 14.5h, cooled to 735°C at a rate of 30°C / h, kept at this temperature for 16.5h, cooled to 350°C and discharged from the furnace;

[0104] 3. Heat treatment process

[0105] (1) Quenching process:

[0106] The forged steel ingot is charged into a furnace for quenching process, specifically: the steel ingot is kept at 230°C for 3 hours, heated to 850°C at a rate of 40°C / h, kept for 4 hours and heated to 1045°C at a rate of 80°C / h, and after being kept for 6.5 hours, the obtained steel ingot is placed in a quenching liquid for quenching, cooled to a maximum temperature of 326°C at the center of the large surface, air-cooled to 86°C, and then charged into a furnace for tempering; when charging into the furnace, the steel ingot should be placed on its side;

[0107] (2) Tempering process:

[0108] After quenching, tempering is immediately carried out, specifically: the quenched steel ingot is heated to 250°C in 6 hours, kept at this temperature for 27 hours, and then air-cooled to obtain plastic mold steel;

[0109] 4. Hardness uniformity

[0110] The plastic mold steel prepared as above was subjected to hardness testing. A portable Leeb hardness tester was used to test the Rockwell hardness. The testing points were located on the diagonal of the end face of the plastic mold steel. A total of 9 points were tested, including the corner, 1 / 4 of the diagonal, and the center. The hardness testing surface required sanding + polishing. The grinding and polishing depth was >4mm for the black leather surface and >1mm for the sawn surface. The results showed that the cross-sectional hardness range of the plastic mold steel was 42~44HRC.

[0111] 5. The performance is shown in Table 4;

[0112] Table 4 Performance data of plastic mold steel prepared in this example

[0113]

[0114] 6. Tissue uniformity

[0115] The metallographic photograph of the core of the plastic mold steel prepared in this embodiment is as follows: Fig.10 As shown by Fig.10 It can be seen that the core structure of the plastic mold steel prepared in this embodiment has good uniformity.

[0116] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0117] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A plastic mold steel, comprising, by mass percentage: C 0.31~0.36%, Si 0.25~0.40%, Mn 0.55~0.80%, Cr 7.50~8.50%, Ni 0.10~0.30%, Mo 0.50~0.70%, V 0.50~0.70%, Al 0.01~0.04%, [N] 0.035~0.045%, and the balance is Fe.

2. The plastic mold steel according to claim 1, characterized in that: The plastic mold steel has P≤0.20%, S≤0.005%, and [O]≤0.0020%.

3. The plastic mold steel according to claim 1, characterized in that: The plastic mold steel comprises: C 0.33-0.35%, Si 0.31-0.39%, Mn 0.62-0.75%, Cr 7.96-8.40%, Ni 0.19-0.28%, Mo 0.62-0.68%, V0.59-0.68%, Al 0.02-0.03%, [N] 0.038-0.042%, P≤0.15%, S≤0.002%, [O]≤0.0015%, and the balance is Fe.

4. The method for preparing the plastic mold steel according to claim 1, comprising the following steps: S1) heating the steel ingot to 550-650°C, heating to 800-900°C after the first heat preservation, heating to 1200-1300°C after the second heat preservation, and then heating for the third time; the composition of the steel ingot is the composition of the plastic mold steel according to any one of claims 1 to 3; S2) forging the steel ingot obtained in step S1) and annealing the forged steel ingot; S3) the steel ingot obtained in step S2) is heated to 800-900°C after the first heat preservation at 200-300°C, heated to 1000-1100°C after the second heat preservation, and quenched after the third heat preservation; S4) The quenched steel ingot is tempered.

5. The preparation method according to claim 4, characterized in that: The forging start temperature is ≥1050°C, and the final forging temperature is ≥850°C; the forging adopts a forging method combining three-time upsetting and FM method, and the FM method forging is started after the three-time upsetting is upset to ≤H0 / 2; H0 is the initial height of the steel ingot.

6. The preparation method according to claim 4, characterized in that: The annealing is specifically: The forged steel ingot is heated from 400~500℃ to 850~900℃ at a rate of 30~50℃ / h, kept at this temperature for 14~17h, then cooled to 720~750℃ at a rate of 10~30℃ / h, kept at this temperature for 16~19h, then cooled to ≤350℃ and taken out of the furnace.

7. The preparation method according to claim 4, characterized in that: In step S3), the quenching cooling method is specifically: The steel ingot is quenched and cooled in the quenching liquid to a maximum temperature of 300~350℃ in the center of the large surface, and then air-cooled to 80~100℃.

8. The preparation method according to claim 4, characterized in that: The tempering treatment is specifically as follows: The quenched steel ingot is heated to 200-300°C, kept at this temperature for 27-36 hours and then air-cooled.

9. The preparation method according to claim 4, characterized in that: In step S1), the first insulation time is 5-7 hours, the heating rate from 550-650°C to 800-900°C is 30-50°C / h, the second insulation time is 6-8 hours, the heating rate from 800-900°C to 1200-1300°C is 70-100°C, and the third insulation time is 20-25 hours.

10. The preparation method according to claim 4, characterized in that: In step S3), the first insulation time is 3-6 hours, the heating rate from 200-300°C to 800-900°C is 10-40°C / h, the second insulation time is 4-6 hours, the heating rate from 800-900°C to 1000-1100°C is 50-80°C / h, and the third insulation time is 0.015D+2-3 hours, where D is the thickness of the forged steel ingot.